Zinc-nickel alloy plating process for aluminum alloy part by taking cyanide-free copper-zinc alloy as bottom plating layer

By replacing the electroless nickel plating layer with cyanide-free copper-zinc alloy process on aluminum alloy parts and using hydroxygraphene modified sealant, the problems of cadmium ion pollution and nickel plating process are solved, and the prevention is improved Corrosion performance and self-repair capability.

CN118979295APending Publication Date: 2024-11-19GUANGZHOU ULTRA UNION CHEM LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411269963.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing aluminum alloys have cadmium ion pollution problems in cadmium plating treatment, and the electroless nickel plating process consumes high energy and costs, and the trivalent chromium passivation film lacks self-repairability, which affects its corrosion resistance.

Method used

The cyanide-free copper-zinc alloy is used as the base coating, and the electroless nickel-plated layer is replaced by the polymerized thiocyanate copper-zinc alloy process, and the self-repairability of the trivalent chromium passivation film is improved by using hydroxygraphene modified sealant.

Benefits of technology

It reduces the risk of cadmium ion pollution, reduces the energy consumption and cost of the nickel plating process, improves the corrosion resistance of zinc-nickel alloy coating, and enhances the self-repairing ability of trivalent chromium passivation film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979295A_ABST
    Figure CN118979295A_ABST
Patent Text Reader

Abstract

The invention discloses a zinc-nickel alloy plating technology for an aluminum alloy part with cyanide-free copper-zinc alloy plating as a bottom plating layer. A chemical zinc deposition layer, a cyanide-free copper-zinc alloy plating layer, a zinc-nickel alloy plating layer, a trivalent chromium passivation film and a hydroxyl graphene modified sealing layer are sequentially prepared on an aluminum alloy matrix from inside to outside. According to the cyanide-free copper-zinc alloy electroplating process, 18-24 g / L of polycuprous thiocyanate, 9-13 g / L of polyzinc thiocyanate, 130-170 g / L of polysodium thiocyanate and 8-12 mL / L of a copper-zinc alloy electroplating brightener are adopted, the pH value of a plating solution is 10-12, the temperature of a plating bath is 35-55 DEG C, the cathode current density is 0.5-1.5 A / dm < 2 >, the cathode movement speed is 3-5 m / min, a brass plate is used as an anode, and the anode movement speed is 3-5 m / min. The surface of a prepared sample piece is free of white rust after being subjected to a neutral salt spray test for 2000 h according to the GB / T 10125-2021 standard, and a plating layer has excellent corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a zinc-nickel alloy plating process for an aluminum alloy part using a cyanide-free copper-zinc alloy as a base plating layer. Background Art

[0002] Aerospace electrical parts are generally made of aluminum alloy and usually need to be cadmium-plated. In the domestic aerospace field, cyanide-free cadmium plating has been widely used instead of cyanide cadmium plating, which effectively reduces the use of cyanide and the pollution to the environment. However, the cadmium pollution problem is still serious. Although the treatment technology of cyanide-free cadmium plating wastewater is mature, due to the high toxicity of cadmium ions, the residual cadmium in the treated wastewater will still cause pollution to the environment.

[0003] In order to reduce cadmium pollution, the industry is developing a new process to replace the cadmium plating with zinc-nickel alloy plating [1] , usually chemical zinc deposition, chemical nickel plating, electroplating of zinc-nickel alloy and chromate passivation are carried out on the aluminum alloy substrate in sequence. The chemical nickel plating layer usually needs to be prepared by a high-temperature chemical nickel plating process, with an operating temperature of about 90°C and excessive energy consumption. The chemical nickel plating solution has a short service life and must be discarded after a period of use, resulting in serious waste of resources. Therefore, the development of new processes with low energy consumption and low material consumption to replace chemical nickel plating has become a trend in the development of technology in this industry.

[0004] The industry has been developing and researching the hexavalent chromium passivation technology for zinc-nickel alloy coatings for many years, but the technology is still not mature enough and needs further research. The technology of using trivalent chromium passivation for zinc-nickel alloy coatings has matured and is widely used in the electroplating production of civilian products. However, the trivalent chromium passivation film does not have self-healing properties, which is a shortcoming in the current anti-corrosion technology. [2] .

[0005] References: [1]. Qin Zhili, Guo Chongwu, Application of high corrosion resistance zinc-nickel alloy protective layer in aerospace field [J], Electroplating & Finishing, 2023, 42(9): 14-17. [2]. Guo Chongwu, Lai Huanwen, Xia Liang, Study on the performance of graphene oxide in coating sealant [J], Electroplating & Finishing, 2021, 40(9): 296-700. Summary of the invention

[0006] In order to solve the problem of high energy consumption and high cost of using chemical nickel plating as the bottom coating of aluminum alloy parts, the present invention provides a zinc-nickel alloy plating process for aluminum alloy parts using cyanide-free copper-zinc alloy plating as the bottom coating. In order to achieve the above purpose, the present invention adopts the following technical solutions: A zinc-nickel alloy plating process for aluminum alloy parts using a cyanide-free copper-zinc alloy as a base plating layer comprises the following steps: (1) Degreasing, film removal, polishing, and micro-corrosion of the aluminum alloy substrate according to the current pre-treatment process; (2) After the aluminum alloy parts are pre-treated, a chemical zinc deposition layer is prepared according to the current chemical zinc deposition process; (3) A cyanide-free copper-zinc alloy coating is prepared by using a polymerized thiocyanate copper-zinc alloy plating process after chemical zinc deposition on aluminum alloy parts; (4) Aluminum alloy parts are plated with copper-zinc alloy by polymerizing thiocyanate and then using the existing zinc-nickel alloy plating process to prepare a zinc-nickel alloy coating; (5) After the aluminum alloy parts are plated with zinc-nickel alloy, the trivalent chromium passivation film is prepared using the current trivalent chromium passivation process; (6) After the aluminum alloy is passivated with trivalent chromium, a hydroxy graphene modified sealing agent is used to prepare a hydroxy graphene modified sealing layer; The polythiocyanate copper-zinc alloy plating process includes the following components and process parameters: Polymeric cuprous thiocyanate 18-24 g / L, polymeric zinc thiocyanate 9-13 g / L, polymeric sodium thiocyanate 130-170 g / L, copper-zinc alloy electroplating brightener 8-12 mL / L, plating solution pH 10-12, plating tank temperature 35-55 ° C, cathode current density 0.5-1.5 A / dm 2 , the cathode moves 3 to 5 m / min, a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 3 to 5 m / min; The copper-zinc alloy electroplating brightener comprises the following components in weight fractions: 60-100 parts of N,N'-di-n-propylethylenediamine, 10-20 parts of waterborne polyurethane resin, 80-120 parts of polyacrylamide with a molecular weight less than 8000, and 770-870 parts of deionized water.

[0007] In some of the embodiments, the polyacrylamide with a molecular weight less than 8000 in the copper-zinc alloy electroplating brightener includes any one or two of polyacrylamide with a model number of GRO-70, polyacrylamide with a model number of IC-113, polyacrylamide with a model number of IC-125, and polyacrylamide with a model number of IC-213.

[0008] In some of the embodiments, the hydroxy graphene modified sealing layer is prepared using PRODICO 480 graphene modified sealing agent: (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.5 to 3.2 times to prepare a sealing solution; (2) Immerse the aluminum alloy parts after trivalent chromium passivation in the sealing liquid for 5 to 15 seconds, drain them after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy parts with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 70 to 90° C. for 20 to 35 minutes.

[0009] In some of the embodiments, the zinc-nickel alloy coating is prepared by using the Detronzin 1315 alkaline zinc-nickel alloy electroplating process: Zinc 5-10g / L, Nickel 0.7-1.8g / L, Sodium hydroxide 120-140g / L, DETRONZIN 1315 Base auxiliary agent 70-100mL / L, DETRONZIN 1315 Ni zinc nickel additive 10-25mL / L, DETRONZIN 1315 Brightener zinc nickel main brightener 0.5-1.5mL / L, DETRONZIN 1315 LCD zinc nickel low zone additive 0.5-1.5mL / L, plating tank temperature 23-28℃, cathode current density 0.8-2.5A / dm 2 , the cathode moves 3 to 5 m / min.

[0010] In some of the embodiments, the zinc-nickel alloy coating is prepared by using DETRONZIN 1377 acid zinc-nickel alloy electroplating process: Zinc 22-30g / L, Nickel 22-30g / L, Potassium chloride 160-190g / L, Ammonium chloride 45-75g / L, DETRONZIN1377A Base auxiliary agent 10-20mL / L, DETRONZIN 1377B Bri main brightener 0.5-1.5mL / L, DETRONZIN1377C Complex complexing agent 10-20mL / L, DETRONZIN 1377D Additive additive 8-12mL / L, plating tank temperature 27-31℃, plating solution pH 4.6-5.2, cathode current density 0.5-3.5A / dm 2 , the cathode moves 3 to 5 m / min.

[0011] In some of the embodiments, the trivalent chromium passivation film is prepared using TRIROS 344 zinc-nickel blue passivation agent: TRIROS 344A zinc-nickel blue passivator 15-75mL / L, TRIROS 344B zinc-nickel blue passivator 25-100mL / L, passivation solution pH 4.0-4.8, operating temperature 20-30℃, slight air stirring, passivation time 45-90s, stay in the air 15-30s.

[0012] In some of the embodiments, the trivalent chromium passivation film is prepared using TRIROS 343 zinc-nickel blue passivation agent: TRIROS 343 zinc-nickel blue passivator 135-175 mL / L, passivation solution pH 1.8-2.6, operating temperature 30-60°C, immersion time 45-75 s, air stirring.

[0013] In some of the embodiments, the chemical zinc deposition layer is prepared using AZIN-113 acidic aluminum zinc deposition agent: AZIN-113 acidic aluminum zinc precipitation agent 150 ~ 250mL / L, working temperature 15 ~ 30 ℃, bath pH 3.4 ~ 4.5, zinc precipitation time 30 ~ 90s.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The zinc-nickel alloy plating process of the aluminum alloy part of the present invention uses a cyanide-free copper-zinc alloy as the bottom plating layer, and uses a polymerized thiocyanate copper-zinc alloy as the bottom plating layer instead of the chemical nickel plating layer, thereby overcoming the high energy consumption and high cost problems of the current chemical nickel plating; 2. The aluminum alloy parts of the present invention use a zinc-nickel alloy plating process with a cyanide-free copper-zinc alloy as the base plating layer, and use a hydroxy graphene modified sealant to seal the zinc-nickel alloy plating layer passivated with trivalent chromium, thereby overcoming the defect that the trivalent chromium passivation film does not have self-repairing properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings: Figure 1 Schematic diagram of the coating structure of Embodiment 1, Embodiment 2, Embodiment 3 and Embodiment 4 of the present invention; Figure 2 This is a photograph of the aluminum alloy zinc-nickel alloy test piece prepared by the present invention after being subjected to a neutral salt spray test for 2000 hours. DETAILED DESCRIPTION

[0016] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0017] A zinc-nickel alloy plating process for aluminum alloy parts using cyanide-free copper-zinc alloy as a base coating comprises the following steps: pretreatment of an aluminum alloy substrate, and sequentially preparing a chemical zinc deposition layer, a polymerized thiocyanate copper-zinc alloy coating, a zinc-nickel alloy coating, a trivalent chromium passivation film, and a hydroxy graphene modified sealing layer on the aluminum alloy substrate from the inside to the outside.

[0018] The existing pre-treatment process is used to remove oil, film, polish and micro-corrosion from the aluminum alloy substrate.

[0019] After the aluminum alloy parts are pre-treated, the chemical zinc deposition layer is prepared by using the current aluminum alloy chemical zinc deposition agent.

[0020] Preferably, the chemical zinc deposition layer is prepared using AZIN-113 acidic aluminum zinc deposition agent produced by Chaobang Chemical: AZIN-113 acidic aluminum zinc precipitation agent 150 ~ 250mL / L, working temperature 15 ~ 30 ℃, bath pH 3.4 ~ 4.5, zinc precipitation time 30 ~ 90s.

[0021] The specific process is: "first zinc precipitation → water washing → zinc stripping → water washing → second zinc precipitation → water washing".

[0022] After chemical zinc deposition on the aluminum alloy part, the polymerized thiocyanate copper-zinc alloy electroplating process of the invention is adopted to prepare the polymerized thiocyanate copper-zinc alloy coating.

[0023] Preferably, the thickness of the polythiocyanate copper-zinc alloy coating is 4-10 μm.

[0024] Polymeric cuprous thiocyanate 18-24 g / L, polymeric zinc thiocyanate 9-13 g / L, polymeric sodium thiocyanate 130-170 g / L, copper-zinc alloy electroplating brightener 8-12 mL / L, plating solution pH 10-12, plating tank temperature 35-55 ° C, cathode current density 0.5-1.5 A / dm 2 The cathode moves at 3 to 5 m / min, and a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 3 to 5 m / min.

[0025] Preferably, the copper-zinc alloy electroplating brightener comprises the following components in weight fractions: 60-100 parts of N,N'-di-n-propylethylenediamine, 10-20 parts of waterborne polyurethane resin, 80-120 parts of polyacrylamide with a molecular weight less than 8000, and 770-870 parts of deionized water.

[0026] Preferably, the polyacrylamide with a molecular weight less than 8000 includes any one or two of polyacrylamide with a model number of GRO-70, polyacrylamide with a model number of IC-113, polyacrylamide with a model number of IC-125, and polyacrylamide with a model number of IC-213.

[0027] Preferably, the copper-zinc alloy electroplating brightener is prepared as follows: 770 to 870 parts by weight of deionized water are added to a reaction tank, 60 to 100 parts of N,N'-di-n-propylethylenediamine, 10 to 20 parts of waterborne polyurethane resin, and 80 to 120 parts of polyacrylamide with a molecular weight less than 8000 are added under stirring, and the brightener is obtained by stirring evenly.

[0028] After the aluminum alloy parts are plated with copper-zinc alloy, the zinc-nickel alloy coating is prepared by the current zinc-nickel alloy plating process.

[0029] Preferably, the zinc-nickel alloy coating has a thickness of 6 to 18 μm.

[0030] Preferably, the zinc-nickel alloy coating is prepared by using the Detronzin 1315 alkaline zinc-nickel alloy electroplating process of Chaobang Chemical: Zinc 5-10g / L, Nickel 0.7-1.8g / L, Sodium hydroxide 120-140g / L, DETRONZIN 1315 Base auxiliary agent 70-100mL / L, DETRONZIN 1315 Ni zinc nickel additive 10-25mL / L, DETRONZIN 1315 Brightener zinc nickel main brightener 0.5-1.5mL / L, DETRONZIN 1315 LCD zinc nickel low zone additive 0.5-1.5mL / L, plating tank temperature 23-28℃, cathode current density 0.8-2.5A / dm 2 , the cathode moves 3 to 5 m / min.

[0031] Preferably, the zinc-nickel alloy coating is prepared by using the DETRONZIN 1377 acid zinc-nickel alloy electroplating process of SuperBang Chemical: Zinc 22-30g / L, Nickel 22-30g / L, Potassium chloride 160-190g / L, Ammonium chloride 45-75g / L, DETRONZIN1377A Base auxiliary agent 10-20mL / L, DETRONZIN 1377B Bri main brightener 0.5-1.5mL / L, DETRONZIN1377C Complex complexing agent 10-20mL / L, DETRONZIN 1377D Additive additive 8-12mL / L, plating tank temperature 27-31℃, plating solution pH 4.6-5.2, cathode current density 0.5-3.5A / dm 2 , the cathode moves 3 to 5 m / min.

[0032] After the aluminum alloy parts are plated with zinc-nickel alloy, the trivalent chromium passivation film is prepared by the current trivalent chromium passivation process.

[0033] Preferably, the trivalent chromium passivation film is prepared using TRIROS 344 zinc-nickel blue passivation agent from Chaobang Chemical: TRIROS 344A zinc-nickel blue passivator 15-75mL / L, TRIROS 344B zinc-nickel blue passivator 25-100mL / L, passivation solution pH 4.0-4.8, operating temperature 20-30℃, slight air stirring, passivation time 45-90s, stay in the air 15-30s.

[0034] Preferably, the trivalent chromium passivation film is prepared using TRIROS 343 zinc-nickel blue passivation agent from Chaobang Chemical: TRIROS 343 zinc-nickel blue passivator 135-175 mL / L, passivation solution pH 1.8-2.6, operating temperature 30-60°C, immersion time 45-75 s, air stirring.

[0035] After trivalent chromium passivation of aluminum alloy parts, PRODICO 480 graphene-modified sealing agent developed by Chaobang Chemical was used to prepare a hydroxy graphene-modified sealing layer.

[0036] Preferably, the thickness of the hydroxy graphene modified sealing layer is 0.8 to 1.4 μm.

[0037] (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.5 to 3.2 times to prepare a sealing solution; (2) Immerse the aluminum alloy parts after trivalent chromium passivation in the sealing liquid for 5 to 15 seconds, drain them after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy parts with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 70 to 90° C. for 20 to 35 minutes.

[0038] Embodiment 1: like Figure 1 As shown, a zinc-nickel alloy plating process for an aluminum alloy part using a cyanide-free copper-zinc alloy as a base coating comprises pre-treatment of an aluminum alloy substrate 1, and sequentially preparing a chemical zinc deposition layer 2, a polymerized thiocyanate copper-zinc alloy coating 3, a zinc-nickel alloy coating 4, a trivalent chromium passivation film 5, and a hydroxy graphene modified sealing layer 6 on the pre-treated aluminum alloy substrate 1 from the inside to the outside.

[0039] 1. Pre-treatment: The aluminum alloy substrate 1 is subjected to "chemical degreasing → water washing → ultrasonic degreasing → water washing → film removal → water washing → light emitting → water washing → micro-corrosion → water washing" by using the current pre-treatment process.

[0040] 2. Chemical zinc precipitation: The chemical zinc deposition layer 2 was prepared using AZIN-113 acidic aluminum zinc deposition agent produced by Chaobang Chemical.

[0041] AZIN-113 acidic aluminum zinc precipitation agent 250mL / L, working temperature 120℃, bath pH 4.0, zinc precipitation time 40s.

[0042] The specific process is: "first zinc precipitation → water washing → zinc stripping → water washing → second zinc precipitation → water washing".

[0043] 3. Copper-zinc alloy: The polythiocyanate copper-zinc alloy electroplating process of the present invention is adopted to prepare the polythiocyanate copper-zinc alloy coating 3, and the coating thickness is 7 μm.

[0044] (1) Preparation of copper-zinc alloy electroplating brightener: The copper-zinc alloy electroplating brightener is prepared as follows: 820 parts of deionized water are added to a reaction tank by weight, 80 parts of N,N'-di-n-propylethylenediamine, 15 parts of waterborne polyurethane resin, and 100 parts of polyacrylamide with a model of GRO-70 are added under stirring, and the brightener is obtained by stirring evenly.

[0045] (2) Plating: Polymeric cuprous thiocyanate 24g / L, polymeric zinc thiocyanate 13g / L, polymeric sodium thiocyanate 170g / L, copper-zinc alloy electroplating brightener 12mL / L, plating solution pH 10, plating tank temperature 35℃, cathode current density 0.8A / dm 2 , the cathode moves at 4m / min, a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 4m / min.

[0046] 4. Zinc-nickel alloy: The zinc-nickel alloy coating 4 was prepared by using the Detronzin 1315 alkaline zinc-nickel alloy electroplating process of Chaobang Chemical, and the coating thickness was 13 μm.

[0047] Zinc 7g / L, Nickel 1.2g / L, Sodium hydroxide 125g / L, DETRONZIN 1315 Base auxiliary agent 100mL / L, DETRONZIN 1315 Ni zinc nickel additive 16mL / L, DETRONZIN 1315 Brightener zinc nickel main brightener 1.0mL / L, DETRONZIN 1315 LCD zinc nickel low zone additive 1.0mL / L, plating tank temperature 23℃, cathode current density 1.2A / dm 2 , cathode moves 4m / min.

[0048] 5. Trivalent chromium passivation: The trivalent chromium passivation film 5 was prepared using TRIROS 344 zinc-nickel blue passivator produced by Chaobang Chemical.

[0049] TRIROS 344A zinc-nickel blue passivator 60mL / L, TRIROS 344B zinc-nickel blue passivator 55mL / L, passivation solution pH 4.2, operating temperature 20℃, slight air stirring, passivation time 50s, air stay 20s.

[0050] 6. Closure: The hydroxy graphene modified sealing layer 6 was prepared by using PRODICO 480 graphene modified sealing agent, and the thickness of the sealing layer was 1.2 μm.

[0051] (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.8 times to prepare a sealing solution; (2) Immerse the aluminum alloy part after trivalent chromium passivation in the sealing liquid for 8 seconds, drain it after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy part with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 85°C for 25 minutes.

[0052] Embodiment 2: like Figure 1 As shown, a zinc-nickel alloy plating process for an aluminum alloy part using a cyanide-free copper-zinc alloy as a base coating comprises pre-treatment of an aluminum alloy substrate 1, and sequentially preparing a chemical zinc deposition layer 2, a polymerized thiocyanate copper-zinc alloy coating 3, a zinc-nickel alloy coating 4, a trivalent chromium passivation film 5, and a hydroxy graphene modified sealing layer 6 on the pre-treated aluminum alloy substrate 1 from the inside to the outside.

[0053] 1. Pre-treatment: The aluminum alloy substrate 1 is subjected to "chemical degreasing → water washing → ultrasonic degreasing → water washing → film removal → water washing → light emitting → water washing → micro-corrosion → water washing" by using the current pre-treatment process.

[0054] 2. Chemical zinc precipitation: The chemical zinc deposition layer 2 was prepared using AZIN-113 acidic aluminum zinc deposition agent produced by Chaobang Chemical.

[0055] AZIN-113 acidic aluminum zinc precipitation agent 150mL / L, working temperature 30℃, bath pH 3.8, zinc precipitation time 70s.

[0056] The specific process is: "first zinc precipitation → water washing → zinc stripping → water washing → second zinc precipitation → water washing".

[0057] 3. Copper-zinc alloy: The polythiocyanate copper-zinc alloy electroplating process of the present invention is adopted to prepare the polythiocyanate copper-zinc alloy coating 3, and the coating thickness is 8 μm.

[0058] (1) Preparation of copper-zinc alloy electroplating brightener: The copper-zinc alloy electroplating brightener is prepared as follows: 820 parts of deionized water are added to a reaction tank by weight, 80 parts of N,N'-di-n-propylethylenediamine, 15 parts of waterborne polyurethane resin, and 100 parts of IC-113 polyacrylamide are added under stirring, and the brightener is obtained by stirring evenly.

[0059] (2) Plating: Polymeric cuprous thiocyanate 17g / L, polymeric zinc thiocyanate 9g / L, polymeric sodium thiocyanate 130g / L, copper-zinc alloy electroplating brightener 8mL / L, plating solution pH 11.5, plating tank temperature 55℃, cathode current density 0.8A / dm 2The cathode moves at 4 m / min, and a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 4 m / min.

[0060] 4. Zinc-nickel alloy: The zinc-nickel alloy coating 4 was prepared by using the Detronzin 1315 alkaline zinc-nickel alloy electroplating process of Chaobang Chemical, and the coating thickness was 12 μm.

[0061] Zinc 10g / L, Nickel 1.8g / L, Sodium hydroxide 130g / L, DETRONZIN 1315 Base 100mL / L, DETRONZIN 1315 Ni 22mL / L, DETRONZIN 1315 Brightener 1.0mL / L, DETRONZIN 1315 LCD low-zone additive 1.0mL / L, bath temperature 23°C, cathode current density 1.6A / dm 2 , cathode moves 4m / min.

[0062] 5. Trivalent chromium passivation: The trivalent chromium blue-white passivation film 5 was prepared using TRIROS 344 zinc-nickel blue passivator produced by Chaobang Chemical.

[0063] TRIROS 344A zinc-nickel blue passivator 60mL / L, TRIROS 344B zinc-nickel blue passivator 85mL / L, passivation solution pH 4.2, operating temperature 20℃, slight air stirring, passivation time 50s, air stay 20s.

[0064] 6. Closure: The hydroxy graphene modified sealing layer 6 was prepared by using PRODICO 480 graphene modified sealing agent, and the thickness of the sealing layer was 1.2 μm.

[0065] (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.8 times to prepare a sealing solution; (2) Immerse the aluminum alloy part after trivalent chromium passivation in the sealing liquid for 10 seconds, drain it after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy part with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 75°C for 35 minutes.

[0066] Embodiment 3: like Figure 1As shown, a zinc-nickel alloy plating process for an aluminum alloy part using a cyanide-free copper-zinc alloy as a base coating comprises pre-treatment of an aluminum alloy substrate 1, and sequentially preparing a chemical zinc deposition layer 2, a polymerized thiocyanate copper-zinc alloy coating 3, a zinc-nickel alloy coating 4, a trivalent chromium passivation film 5, and a hydroxy graphene modified sealing layer 6 on the pre-treated aluminum alloy substrate 1 from the inside to the outside.

[0067] 1. Pre-treatment: The aluminum alloy substrate 1 is subjected to "chemical degreasing → water washing → ultrasonic degreasing → water washing → film removal → water washing → light emitting → water washing → micro-corrosion → water washing" by using the current pre-treatment process.

[0068] 2. Chemical zinc precipitation: The chemical zinc deposition layer 2 was prepared using AZIN-113 acidic aluminum zinc deposition agent produced by Chaobang Chemical.

[0069] AZIN-113 acidic aluminum zinc precipitation agent 240mL / L, working temperature 20℃, bath pH 3.8, zinc precipitation time 50s.

[0070] The specific process is: "first zinc precipitation → water washing → zinc stripping → water washing → second zinc precipitation → water washing".

[0071] 3. Copper-zinc alloy: The polythiocyanate copper-zinc alloy electroplating process of the present invention is adopted to prepare the polythiocyanate copper-zinc alloy coating 3, and the coating thickness is 7 μm.

[0072] (1) Preparation of copper-zinc alloy electroplating brightener: The copper-zinc alloy electroplating brightener is prepared as follows: 820 parts of deionized water are added to a reaction tank by weight, 80 parts of N,N'-di-n-propylethylenediamine, 15 parts of waterborne polyurethane resin, and 100 parts of IC-125 polyacrylamide are added under stirring, and the brightener is obtained by stirring evenly.

[0073] (2) Plating: Polymeric cuprous thiocyanate 20g / L, polymeric zinc thiocyanate 10g / L, polymeric sodium thiocyanate 140g / L, copper-zinc alloy electroplating brightener 10g / L, plating solution pH 11.5, plating tank temperature 40℃, cathode current density 0.8A / dm 2 The cathode moves at 4 m / min, and a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 4 m / min.

[0074] 4. Zinc-nickel alloy: The zinc-nickel alloy coating 4 was prepared by using the DETRONZIN 1377 acid zinc-nickel alloy electroplating process of Chaobang Chemical, and the coating thickness was 13 μm.

[0075] Zinc 26g / L, Nickel 26g / L, Potassium chloride 175g / L, Ammonium chloride 60g / L, DETRONZIN 1377A Base 15mL / L, DETRONZIN 1377B Bri 1.0mL / L, DETRONZIN 1377C Complex 15mL / L, DETRONZIN 1377D Additive 10mL / L, Bath temperature 29°C, Bath pH 4.9, Cathode current density 2.0A / dm 2 , cathode moves 4m / min.

[0076] 5. Trivalent chromium passivation: The trivalent chromium blue-white passivation film 5 was prepared using TRIROS 343 zinc-nickel blue passivator produced by Chaobang Chemical.

[0077] TRIROS 343 zinc-nickel blue passivator 155mL / L, passivation solution pH 2.2, operating temperature 45℃, immersion time 60s, air stirring.

[0078] 6. Closure: The hydroxy graphene modified sealing layer 6 was prepared using PRODICO 480 graphene modified sealing agent developed by Chaobang Chemical, and the thickness of the sealing layer was 1.2 μm.

[0079] (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.8 times to prepare a sealing solution; (2) Immerse the aluminum alloy part after trivalent chromium passivation in the sealing liquid for 12 seconds, drain it after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy part with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 75°C for 35 minutes.

[0080] Embodiment 4: like Figure 1 As shown, a zinc-nickel alloy plating process for an aluminum alloy part using a cyanide-free copper-zinc alloy as a base coating comprises pre-treatment of an aluminum alloy substrate 1, and sequentially preparing a chemical zinc deposition layer 2, a polymerized thiocyanate copper-zinc alloy coating 3, a zinc-nickel alloy coating 4, a trivalent chromium passivation film 5, and a hydroxy graphene modified sealing layer 6 on the pre-treated aluminum alloy substrate 1 from the inside to the outside.

[0081] 1. Pre-treatment: The aluminum alloy substrate 1 is subjected to "chemical degreasing → water washing → ultrasonic degreasing → water washing → film removal → water washing → light emitting → water washing → micro-corrosion → water washing" by using the current pre-treatment process.

[0082] 2. Chemical zinc precipitation: The chemical zinc deposition layer 2 was prepared using AZIN-113 acidic aluminum zinc deposition agent produced by Chaobang Chemical.

[0083] AZIN-113 acidic aluminum zinc precipitation agent 200mL / L, working temperature 25℃, bath pH 4.0, zinc precipitation time 60s.

[0084] The specific process is: "first zinc precipitation → water washing → zinc stripping → water washing → second zinc precipitation → water washing".

[0085] 3. Polythiocyanate copper-zinc alloy plating: The polythiocyanate copper-zinc alloy electroplating process of the present invention is adopted to prepare the polythiocyanate copper-zinc alloy coating 3, and the coating thickness is 8 μm.

[0086] (1) Preparation of copper-zinc alloy electroplating brightener: The copper-zinc alloy electroplating brightener is prepared as follows: 820 parts of deionized water are added to a reaction tank by weight, 80 parts of N,N'-di-n-propylethylenediamine, 15 parts of waterborne polyurethane resin, and 100 parts of IC-213 polyacrylamide are added under stirring, and the brightener is obtained by stirring evenly.

[0087] (2) Plating: Polymeric cuprous thiocyanate 23g / L, polymeric zinc thiocyanate 12g / L, polymeric sodium thiocyanate 160g / L, copper-zinc alloy electroplating brightener 10g / L, plating solution pH 11.5, plating tank temperature 45°C, cathode current density 0.8A / dm 2 , the cathode moves at 4m / min, a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 4m / min.

[0088] 4. Zinc-nickel alloy: The zinc-nickel alloy coating 4 was prepared by using the DETRONZIN 1377 acid zinc-nickel alloy electroplating process of Chaobang Chemical, and the coating thickness was 13 μm.

[0089] 30g / L, nickel 30g / L, potassium chloride 190g / L, ammonium chloride 75g / L, DETRONZIN 1377A Base auxiliary agent 18mL / L, DETRONZIN 1377B Bri main brightener 1.2mL / L, DETRONZIN 1377C Complex complexing agent 18mL / L, DETRONZIN 1377D Additive additive 10mL / L, plating tank temperature 28℃, plating solution pH 5.0, cathode current density 2.0A / dm 2 , cathode moves 4m / min.

[0090] 5. Trivalent chromium passivation: The trivalent chromium blue-white passivation film 5 was prepared using TRIROS 343 zinc-nickel blue passivator produced by Chaobang Chemical.

[0091] TRIROS 343 zinc-nickel blue passivator 175mL / L, passivation solution pH 2.0, operating temperature 35℃, immersion time 60s, air stirring.

[0092] 6. Closure: The hydroxy graphene modified sealing layer 6 was prepared using PRODICO 480 graphene modified sealing agent developed by Chaobang Chemical, and the thickness of the sealing layer was 1.2 μm.

[0093] (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.8 times to prepare a sealing solution; (2) Immerse the aluminum alloy part after trivalent chromium passivation in the sealing liquid for 10 seconds, drain it after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy part with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 80°C for 30 minutes.

[0094] Test Example 1: The effect of the change in the concentration of N,N'-di-n-propylethylenediamine in the copper-zinc alloy electroplating brightener of the present invention on the plated layer was tested.

[0095] Polymerized cuprous thiocyanate 20g / L, polyzinc thiocyanate 11g / L, polysodium thiocyanate 145g / L, plating solution pH 10.5, plating tank temperature 45°C, cathode current density 1.0A / dm 2 , using a copper-zinc alloy plate as the anode. The content of waterborne polyurethane and polyacrylamide with a molecular weight less than 8000 in the brightener takes the middle value of the copper-zinc alloy electroplating brightener formula, and the amount of N,N'-di-n-propylethylenediamine added to the plating solution is 0.2-1.4 g / L. The test shows that the range of the amount of N,N'-di-n-propylethylenediamine added is not wide. The test results show that the concentration of N,N'-di-n-propylethylenediamine in the copper-zinc alloy electroplating brightener is calculated according to the upper and lower limits, and the amount of the copper-zinc alloy electroplating brightener added in the range of 7-13 mL / L can usually obtain a good copper-zinc alloy coating.

[0096] Table 1, Effect of the amount of N,N'-di-n-propylethylenediamine added on the quality of the coating Test Example 2: The influence of the concentration change of the waterborne polyurethane resin in the copper-zinc alloy electroplating brightener of the present invention on the plated layer was tested.

[0097] Polymerized cuprous thiocyanate 20g / L, polyzinc thiocyanate 11g / L, polysodium thiocyanate 145g / L, plating solution pH 10.5, plating tank temperature 45°C, cathode current density 1.0A / dm 2, using a copper-zinc alloy plate as the anode. The addition amount of N,N'-di-n-propylethylenediamine and polyacrylamide with a molecular weight less than 8000 is taken as the middle value of the formula, and the addition amount of waterborne polyurethane resin in the plating solution is 0.01-0.40g / L. The test shows that the concentration of waterborne polyurethane resin in the copper-zinc alloy electroplating brightener is calculated according to the upper and lower limits, and the addition amount of the copper-zinc alloy electroplating brightener in the range of 5-17mL / L can obtain a good copper-zinc alloy coating.

[0098] Table 2, Effect of the amount of waterborne polyurethane resin added on the quality of the coating Waterborne polyurethane resin (g / L) Coating color Plating gloss 0.01 Brass Not bright 0.05 Brass Brightness is acceptable 0.10 Brass Brighter 0.15 Brass Brighter 0.20 Brass Brighter 0.25 Brass Brighter 0.30 Brass Brighter 0.35 Brass Brighter 0.40 Brass Brighter, poorer positioning Test Example 3: The influence of the concentration change of polyacrylamide with a molecular weight less than 8000 in the copper-zinc alloy electroplating brightener of the present invention on the plated layer was tested.

[0099] Polymerized cuprous thiocyanate 20g / L, polyzinc thiocyanate 11g / L, polysodium thiocyanate 145g / L, plating solution pH 10.5, plating tank temperature 45°C, cathode current density 1.0A / dm 2 , using copper-zinc alloy plate as anode. The amount of waterborne polyurethane and N,N'-di-n-propylethylenediamine added to the plating solution is the middle value of the formula, and the amount of polyacrylamide with a molecular weight less than 8000 added to the plating solution is 0.2-2.0 g / L. The test shows that the range of the amount of polyacrylamide with a molecular weight less than 8000 is relatively wide. According to the upper and lower limits of the concentration of polyacrylamide with a molecular weight less than 8000 in the copper-zinc alloy electroplating brightener, the amount of the brightener added in the range of 5-17 mL / L can obtain a good copper-zinc alloy coating.

[0100] Table 3, Effect of the amount of polyacrylamide added with a molecular weight less than 8000 on the quality of the coating Waterborne polyurethane resin (g / L) Coating color Plating gloss 0.2 Brass Not bright enough 0.4 Brass Brighter 0.6 Brass Brighter 0.8 Brass Brighter 1.0 Brass Brighter 1.2 Brass Brighter 1.4 Brass Brighter 1.6 Brass Brighter 1.8 Brass Brighter 2.0 Brass Brighter The comprehensive test results of Test Examples 1-3 show that, based on the concentration of the components contained in the copper-zinc alloy electroplating brightener calculated according to the upper and lower limits, a good copper-zinc alloy plating layer can usually be obtained when the addition amount of the brightener is within the range of 7 to 13 mL / L.

[0101] Test example 4: A 40mm×60mm×2mm aluminum alloy test piece was electrolessly zinc-plated, copper-zinc alloy-plated, zinc-nickel alloy-plated, blue-white passivation with trivalent chromium, and sealed with a hydroxy graphene modified sealant according to this process. The thickness of the copper-zinc alloy coating was 8μm, the zinc-nickel alloy coating was 12μm, and the thickness of the hydroxy graphene modified sealing layer was 1.2μm. According to the standard GB / T 10125-2021 "Artificial Atmosphere Corrosion Test Salt Spray Test", a neutral salt spray test was carried out for 2000h. There was no white rust on the surface of the sample. The test results are as follows: Figure 2 shown.

[0102] Test Example 5: The zinc-nickel alloy samples on the surface of the aluminum alloy prepared in Example 1, Example 2, Example 3 and Example 4 were tested for the bonding strength of the coating in accordance with GB / T 5270-2005 "Review of test methods for adhesion strength of electrodeposited and chemically deposited metal coatings on metal substrates". The zinc-nickel alloy samples on the surface of the aluminum alloy were placed in a heating furnace and heated to 220°C for 30 minutes. After being taken out, they were quenched in water at room temperature. There was no blistering or shedding of the coating, and the coating bonding strength met the standard requirements.

[0103] The technical solutions provided by the embodiments of the present invention are described in detail above. The principles and implementation methods of the embodiments of the present invention are described in detail using specific examples herein. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which are also considered to fall within the protection scope of the present invention.

Claims

1. A zinc-nickel alloy plating process for aluminum alloy parts using cyanide-free copper-zinc alloy as the bottom plating layer, characterized in that: The following steps are involved: (1) Degreasing, film removal, polishing, and micro-corrosion of the aluminum alloy substrate according to the current pre-treatment process; (2) After the aluminum alloy parts are pre-treated, a chemical zinc deposition layer is prepared according to the current chemical zinc deposition process; (3) A cyanide-free copper-zinc alloy coating is prepared by using a polymerized thiocyanate copper-zinc alloy plating process after chemical zinc deposition on aluminum alloy parts; (4) Aluminum alloy parts are plated with copper-zinc alloy by polymerizing thiocyanate and then using the existing zinc-nickel alloy plating process to prepare a zinc-nickel alloy coating; (5) After the aluminum alloy parts are plated with zinc-nickel alloy, the trivalent chromium passivation film is prepared using the current trivalent chromium passivation process; (6) After the aluminum alloy is passivated with trivalent chromium, a hydroxy graphene modified sealing agent is used to prepare a hydroxy graphene modified sealing layer; The polythiocyanate copper-zinc alloy plating process includes the following components and process parameters: Polymeric cuprous thiocyanate 18-24 g / L, polymeric zinc thiocyanate 9-13 g / L, polymeric sodium thiocyanate 130-170 g / L, copper-zinc alloy electroplating brightener 8-12 mL / L, plating solution pH 10-12, plating tank temperature 35-55 ° C, cathode current density 0.5-1.5 A / dm 2 , the cathode moves 3 to 5 m / min, a copper-zinc alloy plate with a copper mass fraction of 68% is used as the anode, and the anode moving speed is 3 to 5 m / min; The copper-zinc alloy electroplating brightener comprises the following components in weight fractions: 60-100 parts of N,N'-di-n-propylethylenediamine, 10-20 parts of waterborne polyurethane resin, 80-120 parts of polyacrylamide with a molecular weight less than 8000, and 770-870 parts of deionized water.

2. The zinc-nickel alloy plating process for aluminum alloy parts according to claim 1, wherein the zinc-nickel alloy plating process uses a cyanide-free copper-zinc alloy as a bottom plating layer, characterized in that: The polyacrylamide with a molecular weight less than 8000 in the copper-zinc alloy electroplating brightener includes any one or two of polyacrylamide with a model number of GRO-70, polyacrylamide with a model number of IC-113, polyacrylamide with a model number of IC-125, and polyacrylamide with a model number of IC-213.

3. The zinc-nickel alloy plating process for aluminum alloy parts according to claim 1, wherein the zinc-nickel alloy plating process uses a cyanide-free copper-zinc alloy as a bottom plating layer, characterized in that: The hydroxy graphene modified sealing layer is prepared using PRODICO 480 graphene modified sealing agent: (1) Dilute PRODICO 480 graphene-modified sealer with water to 2.5 to 3.2 times to prepare a sealing solution; (2) Immerse the aluminum alloy parts after trivalent chromium passivation in the sealing liquid for 5 to 15 seconds, drain them after exiting the tank, and blow off the sealing liquid remaining on the surface of the aluminum alloy parts with high-pressure air; (3) The sealed aluminum alloy parts are dried and cured at 70 to 90° C. for 20 to 35 minutes.

4. The zinc-nickel alloy plating process for aluminum alloy parts according to claim 1, wherein the zinc-nickel alloy plating process uses a cyanide-free copper-zinc alloy as a bottom plating layer, characterized in that: The zinc-nickel alloy coating is prepared by using the Detronzin 1315 alkaline zinc-nickel alloy electroplating process: Zinc 5-10g / L, Nickel 0.7-1.8g / L, Sodium hydroxide 120-140g / L, DETRONZIN 1315 Base auxiliary agent 70-100mL / L, DETRONZIN 1315 Ni zinc nickel additive 10-25mL / L, DETRONZIN 1315 Brightener zinc nickel main brightener 0.5-1.5mL / L, DETRONZIN 1315 LCD zinc nickel low zone additive 0.5-1.5mL / L, plating tank temperature 23-28℃, cathode current density 0.8-2.5A / dm 2 , the cathode moves 3 to 5 m / min.

5. The zinc-nickel alloy plating process for aluminum alloy parts with cyanide-free copper-zinc alloy as the bottom plating layer as claimed in claim 1, characterized in that: The zinc-nickel alloy coating is prepared by using the DETRONZIN 1377 acidic zinc-nickel alloy electroplating process: Zinc 22-30g / L, Nickel 22-30g / L, Potassium chloride 160-190g / L, Ammonium chloride 45-75g / L, DETRONZIN 1377ABase auxiliary agent 10-20mL / L, DETRONZIN 1377B Bri main brightener 0.5-1.5mL / L, DETRONZIN 1377CComplex complexing agent 10-20mL / L, DETRONZIN 1377D Additive additive 8-12mL / L, plating tank temperature 27-31℃, plating solution pH 4.6-5.2, cathode current density 0.5-3.5A / dm 2 , the cathode moves 3 to 5 m / min.

6. The zinc-nickel alloy plating process for aluminum alloy parts with cyanide-free copper-zinc alloy as the bottom plating layer as claimed in claim 1, characterized in that: The trivalent chromium passivation film is prepared using TRIROS 344 zinc-nickel blue passivation agent: TRIROS 344A zinc-nickel blue passivator 15-75mL / L, TRIROS 344B zinc-nickel blue passivator 25-100mL / L, passivation solution pH 4.0-4.8, operating temperature 20-30℃, slight air stirring, passivation time 45-90s, stay in the air 15-30s.

7. The zinc-nickel alloy plating process for aluminum alloy parts with cyanide-free copper-zinc alloy as the bottom plating layer as claimed in claim 1, characterized in that: The trivalent chromium passivation film is prepared using TRIROS 343 zinc-nickel blue passivation agent: TRIROS 343 zinc-nickel blue passivator 135-175 mL / L, passivation solution pH 1.8-2.6, operating temperature 30-60°C, immersion time 45-75 s, air stirring.

8. The zinc-nickel alloy plating process for aluminum alloy parts with cyanide-free copper-zinc alloy as the bottom plating layer as claimed in claim 1, characterized in that: The chemical zinc deposition layer is prepared by using AZIN-113 acidic aluminum zinc deposition agent: AZIN-113 acidic aluminum zinc precipitation agent 150 ~ 250mL / L, working temperature 15 ~ 30 ℃, bath pH 3.4 ~ 4.5, zinc precipitation time 30 ~ 90s.

Citation Information

Cited By

  • Neodymium-iron-boron cyanide-free cadmium-iron alloy plating process suitable for aerospace field

    CN119592937A