Method for modifying diaphragm and lithium-sulfur battery based on metal organic framework defect structure

By using metal organic frame defects to construct the modified separator in lithium sulfur batteries, the problem of LiPSs shuttle effect in lithium sulfur batteries is solved, the cycle stability and energy efficiency of the battery are improved, and the performance of the separator is enhanced.

CN118983613AActive Publication Date: 2024-11-19SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202411022357.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-19
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The LiPSs shuttle effect generated by lithium-sulfur batteries during charging and discharging leads to performance instability and safety risks, and existing diaphragm materials cannot effectively suppress this problem.

Method used

Using a modified separator based on defects in metal organic frames, the defective metal organic frame material is synthesized by solvent thermal method, mixed with conductive agent and binder, coated on traditional separator to form a modified separator to improve lithium ion transport Channels and LiPSs adsorption sites to reduce side reactions.

Benefits of technology

It significantly inhibits the shuttle effect of LiPSs, improves the reversible capacity, cycle stability and energy efficiency of lithium-sulfur batteries, enhances the flexibility and conductivity of the membrane, reduces structural damage, and promotes the redox reaction of LiPSs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983613A_ABST
    Figure CN118983613A_ABST
Patent Text Reader

Abstract

The invention discloses a method for constructing a modified diaphragm based on metal organic framework defects, which comprises the following steps: firstly, synthesizing a defective metal organic framework crystal material with adjustable porosity, high specific surface area and potential catalytic performance by adopting a solvothermal method; the material is mixed with a conductive agent and a binder according to a certain proportion to prepare uniform slurry, and the slurry is coated on a PP diaphragm through a blade coating process to obtain the metal organic framework material modified diaphragm with defects. The modified diaphragm not only has a high specific surface area, but also provides sufficient ion conduction channels to limit the diffusion of LiPSs, has good electro-catalysis capability, and promotes LiPSs conversion kinetics under a poor electrolyte condition. The modified diaphragm, the S-coated CNT composite positive electrode material and the metal lithium sheet negative electrode material are assembled into the lithium-sulfur battery, so that the lithium-sulfur battery has excellent cycling stability and low impedance characteristic, the energy density of the battery is improved, and the service life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of energy storage battery materials, and in particular relates to a method for modifying a diaphragm based on a metal organic framework defect structure, and also relates to a method for preparing a lithium sulfur battery. Background Art

[0002] Faced with the environmental and energy crisis caused by non-renewable fossil fuels and the instability of renewable energy output, the development of secondary battery technology is particularly important. Lithium-sulfur batteries (LSBs) are particularly prominent, which not only have high theoretical specific capacity (1675mAh·g-1) and high energy density (2600Wh·kg-1), but also have abundant sulfur resources as cathode materials, making them a rising star with great development potential in the field of energy storage. Despite the bright prospects, the application of LSBs still faces major obstacles: the side reaction between metallic lithium and electrolyte generates lithium dendrites, which triggers safety risks. In addition, the shuttle effect of polysulfides (LiPSs) is another major problem restricting the commercial application of LSBs. In order to overcome the above challenges, researchers are committed to optimizing the sulfur cathode structure, electrolyte composition and diaphragm materials to improve battery performance and safety.

[0003] The separator is extremely critical to improving the performance of LSBs. The separator not only prevents the positive and negative electrodes from contacting, but also ensures the smooth transmission of lithium ions. At present, the commonly used commercial separator materials in lithium-sulfur batteries are polypropylene (PP) and polyethylene (PE). Such separators have problems such as easy curling when heated, poor mechanical properties, and large pores that cannot inhibit the LiPSs generated during charging and discharging, which seriously affect the performance of lithium-sulfur batteries. In recent years, researchers have significantly inhibited the shuttle effect of LiPSs by modifying the separator. Therefore, careful design and optimization of the separator can significantly improve the reversible capacity, Coulomb efficiency and cycle stability of LSBs. Defective metal-organic frameworks (MOFs) have become ideal materials for modified separator coatings due to their unique structure, adjustable porosity, high specific surface area and potential catalytic performance. MOFs can optimize the ion transmission path by controlling defects, while providing effective adsorption sites and catalytic active centers for LiPSs, which can inhibit the shuttle effect and thus improve the performance of the battery. Summary of the invention

[0004] The first objective of the present invention is to provide a method for modifying a diaphragm based on a metal organic framework defect structure, which solves the problem that traditional lithium sulfur batteries cannot suppress the LiPSs shuttle effect generated during the charge and discharge process.

[0005] The second object of the present invention is to provide a modified membrane based on the defect structure of metal organic framework.

[0006] The third object of the present invention is to provide a method for preparing a lithium-sulfur battery.

[0007] The first technical solution adopted by the present invention is a method for modifying the diaphragm based on the defects of the metal organic framework, and the specific operation steps are as follows:

[0008] Step 1: Weigh a certain amount of thiophene-2-carboxylic acid (C9H6O2S2), 5-methyltetrazole (C2H4N4) and zinc nitrate hexahydrate (Zn(NO3)2·6H2O), add to a mixed solution of methanol (CH4O) and N,N-dimethylacetamide (DMA), stir at room temperature, then add 2,5-thiophenedicarboxylic acid (C6H4O4S) and continue stirring until dissolved, finally add 1 drop of tetramethylammonium hydroxide solution, put into a reactor at 120°C for 2 days, cool to room temperature, wash three times with DMA, and dry to obtain a defective metal organic framework crystal material A;

[0009] Step 2: Grind the defective crystal material A and the conductive agent obtained in step 1 evenly, then add a binder and N-methylpyrrolidone (NMP) solution and stir to form a uniform slurry B;

[0010] Step 3: Use a 100° scraper to evenly coat the slurry B obtained in step 2 on the surface of the PP diaphragm, and then place the diaphragm in a 60°C vacuum drying oven to dry, thereby obtaining a modified diaphragm C;

[0011] Step 4: Cut the modified diaphragm C in step 3 into a circle using a 19 mm punch to obtain a modified battery diaphragm D.

[0012] The present invention is also characterized in that:

[0013] The thiophene-2-carboxylic acid in step 1 can be replaced by any one of 2-chlorothiophene-5-carboxylic acid and 5-bromo-2-carboxythiophene; the molar ratio of 2,5-thiophenedicarboxylic acid to thiophene-2-carboxylic acid, 2-chlorothiophene-5-carboxylic acid and 5-bromo-2-carboxythiophene is 9 to 1:1;

[0014] Step 1: The mass ratio of the defective crystal material A synthesized in step 2 in the conductive agent and the binder is not less than 50%, and the mixture is stirred for at least 30 minutes.

[0015] The conductive agent in step 2 can be replaced by any one of Super P, graphene and Ketjen black; the binder can be replaced by any one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE) and polyethylene oxide (PEO).

[0016] In step 3, the coating thickness of the modified diaphragm C is 50 to 150 nm.

[0017] The vacuum drying temperature in step 3 is 55°C to 70°C, and the drying time is not less than 12 hours.

[0018] In step 4, the diameter of the cut piece of battery separator is 19 mm. The size of the soft-pack battery separator can be cut according to the soft-pack shell.

[0019] The second technical solution adopted by the present invention is: a modified diaphragm based on a metal organic framework defect structure is prepared by a method for modifying a diaphragm based on a metal organic framework defect structure.

[0020] The third technical solution adopted by the present invention is: a method for preparing a lithium-sulfur battery, assembling a modified diaphragm D with a S@CNT composite positive electrode material, a metal lithium sheet negative electrode material spring and a gasket in a glove box to form a lithium-sulfur battery; the S@CNT composite positive electrode material is a composite positive electrode material made by loading sulfur on carbon nanotubes.

[0021] The battery cycle, rate, impedance and CV curve were tested at different currents; different current densities included 0.1C, 0.2C, 0.5C, 1C, and 2C; the parameter frequency for electrochemical impedance spectroscopy was 0.01-1000000Hz, the cyclic voltammetry test voltage was 1.6V-2.8V, and the scan rate was 0.0001V / s-0.0005V / s.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present invention prepares a metal organic framework material A with defects by a solvothermal method. The defects can change the pore size and shape of MOFs, provide a more optimized channel for the transmission of lithium ions and LiPSs, and reduce the occurrence of side reactions.

[0024] (2) An appropriate number of defects can increase the structural flexibility of MOFs, allowing them to better adapt to volume changes during charge and discharge and reduce structural damage. The introduction of polar groups during the defect construction process can improve the interfacial compatibility between MOFs and electrolytes, further improving battery performance.

[0025] (3) Benefiting from the synergistic advantages of defective MOFs-modified separators, the appropriate porous structure shows good screening ability in preventing the adverse migration of LiPSs, while the large surface area is conducive to the rapid transfer of electrons and ions. Specific defect sites can act as catalysts to promote the redox reaction of LiPSs and improve the cycle stability and energy efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a flow chart of the preparation of a modified diaphragm based on a metal organic framework defect structure of the present invention;

[0027] Figure 2 It is an X-ray diffraction pattern of the crystal material based on the metal organic framework defect structure of the present invention;

[0028] Figure 3 is a graph showing the relationship between current density and potential (CV) of the lithium-sulfur battery of the present invention;

[0029] Figure 4 is the electrochemical impedance spectroscopy (EIS) of the lithium-sulfur battery of the present invention;

[0030] Figure 5 It is a relationship diagram between efficiency and specific capacity of the lithium-sulfur battery of the present invention at a current density of 0.1C. DETAILED DESCRIPTION

[0031] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0032] The method for modifying a diaphragm based on a metal organic framework defect structure provided by the present invention comprises the synthesis of a metal organic framework defect material, mixing the defect crystal material with a conductive agent (Super P) and a binder (PVDF) to prepare a slurry which is then scraped onto a PP diaphragm to obtain a modified diaphragm; finally, the modified diaphragm is assembled with a S@CNT composite positive electrode material and a metal lithium negative electrode material into a lithium-sulfur battery.

[0033] Example 1

[0034] The method for modifying the diaphragm based on the metal organic framework defect structure provided by the present invention is as follows: Figure 1 The specific steps are as follows:

[0035] Step 1: Weigh thiophene-2-carboxylic acid (0.029 mmol, 0.004 g), 5-methyltetrazole (1.2 mmol, 0.102 g) and zinc nitrate hexahydrate (0.54 mmol, 0.160 g), add to a mixed solution of N, N-dimethylacetamide (3 mL) and methanol (3 mL), stir evenly at room temperature, then add 2,5-thiophenedicarboxylic acid (0.261 mmol, 0.045 g) and stir until dissolved, add 1 drop of tetramethylammonium hydroxide, put into a reactor, react in an oven at 120° C. for 2 days, cool to room temperature, wash three times with DMA, and dry to obtain a metal organic framework material with defects, recorded as light yellow crystal A;

[0036] Step 2: Weigh 0.07 g, 0.02 g and 0.01 g of the light yellow crystal A obtained in step 1, a conductive agent (Super P) and a binder (PVDF) in a mass ratio of 7:2:1, add NMP and stir for 30 min to prepare a uniform viscous slurry B;

[0037] Step 3: Use a 75 μm scraper to evenly scrape the slurry B obtained in step 2 on the surface of the diaphragm, and then dry the diaphragm in a vacuum drying oven at 65° C. for 12 hours to obtain a modified diaphragm C;

[0038] Step 4: Cut the modified separator C obtained in step 3 into a circle using a punch with a diameter of 19 mm to obtain a modified battery separator D;

[0039] Step 5: Assemble the battery separator D obtained in step 4 with the S@CNT composite positive electrode material, the metal lithium sheet negative electrode material, the spring, and the gasket into a lithium-sulfur battery in a glove box, and test the cycle, rate (0.1C, 0.2C, 0.5C, 1C, 2C), impedance (frequency of 0.01-1000000 Hz), and CV (1.6V-2.8V, scan rate of 0.0001V / s-0.0005V / s) at different currents.

[0040] Example 2

[0041] Step 1: Weigh thiophene-2-carboxylic acid (0.09 mmol, 0.011 g), 5-methyltetrazole (1.2 mmol, 0.102 g) and zinc chloride (0.54 mmol, 0.0073 g), add to a mixed solution of DMA (4 mL) and methanol (4 mL), stir at room temperature until the solution is uniform and transparent, then add 2,5-thiophenedicarboxylic acid (0.2 mmol, 0.035 g) and stir until dissolved, add 1 drop of tetramethylammonium hydroxide, put into a reactor, react in an oven at 100 ° C for 3 days, cool to room temperature, wash three times with DMA, and dry to obtain a defective metal organic framework material as light yellow crystal A;

[0042] Step 2: 0.06 g, 0.02 g and 0.01 g of the light yellow crystal A obtained in step 1, a conductive agent (Ketjen black) and a binder (PVDF) were weighed in a ratio of 6:2:1, respectively, and NMP was added and stirred for 30 min to prepare a uniform viscous slurry B;

[0043] Step 3: Use a 75 μm scraper to evenly scrape the slurry B obtained in step 2 on the surface of the diaphragm, and then dry the diaphragm in a vacuum drying oven at 50° C. for 15 hours to obtain a modified diaphragm C;

[0044] Step 4: Cut the modified separator C obtained in step 3 into a circle using a punch with a diameter of 19 mm to obtain a modified battery separator D;

[0045] Step 5: Assemble the battery separator D obtained in step 4 with the S@CNT composite positive electrode material, the metal lithium sheet negative electrode material, the spring, and the gasket into a lithium-sulfur battery in a glove box, and test the cycle, rate (0.1C, 0.2C, 0.5C, 1C, 2C), impedance (frequency of 0.01-1000000 Hz), and CV (1.6V-2.8V, scan rate of 0.0001V / s-0.0005V / s) at different currents.

[0046] Example 3

[0047] Step 1: Weigh thiophene-2-carboxylic acid (0.145 mmol, 0.019 g), 5-methyltetrazole (1.2 mmol, 0.102 g) and zinc acetate dihydrate (0.54 mmol, 0.118 g), add to a mixed solution of N,N-dimethylacetamide DMA (3 mL) and methanol (3 mL), stir at room temperature until the solution is uniform and transparent, then add 2,5-thiophenedicarboxylic acid (0.145 mmol, 0.025 g) and stir until dissolved, add 1 drop of tetramethylammonium hydroxide, put into a reactor, react in an oven at 120° C. for 3 days, cool to room temperature, wash three times with DMA, and dry to obtain a metal organic framework material with defects, recorded as light yellow crystal A;

[0048] Step 2: weigh 0.08 g, 0.01 g and 0.01 g of the light yellow crystal A obtained in step 1, a conductive agent (Super P) and polytetrafluoroethylene (PTFE) in a ratio of 8:1:1, respectively, add NMP and stir for 30 min to prepare a uniform viscous slurry B;

[0049] Step 3: Use a 100 μm scraper to evenly scrape the slurry B obtained in step 2 on the surface of the diaphragm, and then dry the diaphragm in a vacuum drying oven at 70° C. for 12 hours to obtain a modified diaphragm C;

[0050] Step 4: Cut the modified separator C obtained in step 3 into a circle using a punch with a diameter of 19 mm to obtain a modified battery separator D;

[0051] Step 5: Assemble the battery separator D obtained in step 4 with the S@CNT composite positive electrode material, the metal lithium sheet negative electrode material, the spring, and the gasket into a lithium-sulfur battery in a glove box, and test the cycle, rate (0.1C, 0.2C, 0.5C, 1C, 2C), impedance (frequency of 0.01-1000000 Hz), and CV (1.6V-2.8V, scan rate of 0.0001V / s-0.0005V / s) at different currents.

[0052] Example 4

[0053] Step 1: Weigh thiophene-2-carboxylic acid (0.145 mmol, 0.019 g), 5-methyltetrazole (1.2 mmol, 0.102 g), and zinc chloride (0.54 mmol, 0.073 g), add to a mixed solution of DMA (6 mL) and methanol (6 mL), stir at room temperature until the solution is uniform and transparent, then add 2,5-thiophenedicarboxylic acid (0.145 mmol, 0.025 g) and stir until dissolved, add 1 drop of tetramethylammonium hydroxide, put into a reactor, react in an oven at 140° C. for 2 days, cool to room temperature, wash three times with DMA solution, and dry to obtain a metal organic framework material with defects, recorded as light yellow crystal A;

[0054] Step 2: 0.07 g, 0.02 g and 0.01 g of the light yellow crystal A obtained in step 1, a conductive agent (Super P) and polyethylene oxide (PEO) were weighed in a ratio of 7:2:1, respectively, and NMP solution was added and stirred for 30 min to prepare a uniform viscous slurry B;

[0055] Step 3: Use a 75 μm scraper to evenly scrape the slurry B obtained in step 2 on the surface of the diaphragm, and then dry the diaphragm in a vacuum drying oven at 65° C. for 12 hours to obtain a modified diaphragm C;

[0056] Step 4: Cut the modified separator C obtained in step 3 into a circle using a punch with a diameter of 19 mm to obtain a modified battery separator D;

[0057] Step 5: Assemble the battery separator D obtained in step 4 with the S@CNT composite positive electrode material, the metal lithium sheet negative electrode material, the spring, and the gasket into a lithium-sulfur battery in a glove box, and test the cycle, rate (0.1C, 0.2C, 0.5C, 1C, 2C), impedance (frequency of 0.01-1000000 Hz), and CV (1.6V-2.8V, scan rate of 0.0001V / s-0.0005V / s) at different currents.

[0058] Example 5

[0059] Step 1: Weigh thiophene-2-carboxylic acid (0.09 mmol, 0.011 g), 5-methyltetrazole (1.2 mmol, 0.102 g) and zinc nitrate hexahydrate (0.54 mmol, 0.160 g), add to a mixed solution of DMA (3 mL) and methanol (3 mL), stir at room temperature until the solution is uniform and transparent, then add 2,5-thiophenedicarboxylic acid (0.2 mmol, 0.035 g) and stir until dissolved, add 1 drop of tetramethylammonium hydroxide, put into a reactor, react in an oven at 120° C. for 2 days, cool to room temperature, wash three times with DMA, and dry to obtain a metal organic framework material with defects, recorded as light yellow crystal A;

[0060] Step 2: weigh 0.07 g, 0.02 g and 0.01 g of the light yellow crystal A obtained in step 1, the conductive agent (graphene) and the binder (PVDF) in a ratio of 7:2:1, respectively, add NMP and stir for 30 min to prepare a uniform viscous slurry B;

[0061] Step 3: Use a 125 μm scraper to evenly scrape the slurry B obtained in step 2 on the surface of the diaphragm, and then dry the diaphragm in a vacuum drying oven at 65° C. for 12 hours to obtain a modified diaphragm C;

[0062] Step 4: Cut the modified separator C obtained in step 3 into a square of 5 cm×5 cm to obtain a modified battery separator D;

[0063] Step 5: The battery separator D obtained in step 4 was assembled into a lithium-sulfur soft pack battery in a glove box with the S@CNT composite positive electrode material cut into 4.5cm×4.5cm, the metal lithium sheet negative electrode material, the positive electrode ear, the negative electrode ear and the aluminum-plastic packaging bag. The cycle, rate (0.1C, 0.2C, 0.5C, 1C, 2C), impedance (frequency 0.01-1000000Hz), and CV (1.6V-2.8V, scan rate 0.0001V / s-0.0005V / s) were tested at different currents.

[0064] like Figure 2 The figure shows the X-ray diffraction pattern of the defective structure of the metal organic framework. According to the XRD pattern, the crystal peaks of the defective crystal material are basically consistent with the standard curve, indicating that the metal organic framework defective material has been successfully synthesized.

[0065] like Figure 3 The figure shows the relationship between current density and potential of a lithium-sulfur battery assembled with a metal organic framework material defect structure modified diaphragm at a scan rate of 0.0001V / s. It can be seen from the figure that between 1.6V-2.8V, the curve shows an obvious peak current, indicating that a sulfur redox reaction occurred in the process. During the discharge process, the reduction peak near 2.2V-2.4V corresponds to the reduction of S8 to soluble Li2S n (4≤n≤8), the reduction peak around 1.9V-2.1V corresponds to Li2S n Further reduced to Li2S2 and Li2S. During the charging process, the oxidation peak near 2.4V-2.6V corresponds to the conversion of Li2S2 and Li2S into soluble Li2S n And eventually transformed into S8.

[0066] like Figure 4 As shown, it is the electrochemical impedance diagram of the lithium-sulfur battery assembled with the metal organic framework defect structure diaphragm of the present invention. It is a semicircle in the high frequency region and approximately a straight line in the low frequency region. The intercept of the semicircle represents the solution resistance of the electrolyte, the semicircle represents the charge transfer impedance, and the oblique line is related to the Warburg impedance of ion diffusion during the charge and discharge process. It can be seen from the figure that the semicircle has a smaller diameter and has a lower electrode polarization impedance. This is due to the high conductivity of the modified diaphragm, which accelerates the transmission of electrons and ions to the sulfur positive electrode.

[0067] like Figure 5 The figure shows the specific capacity cycle diagram of the lithium-sulfur battery assembled with the metal organic framework defect structure diaphragm of the present invention. The lithium-sulfur battery assembled with the modified diaphragm has a specific capacity of 1531.7 mAh·g at 0.1C.-1 Initial capacity: 653.4 mAh g after 50 cycles -1 The discharge capacity of the LiPSs is 100%, and the corresponding capacity retention rate is approximately 100%. This indicates that the modified separator with defective structure of metal organic framework can promote the transmission of lithium ions and effectively inhibit the shuttle effect of LiPSs.

[0068] The synthesis principle of the key steps in the present invention is:

[0069] (1) The defect structure of the present invention is to synthesize materials containing organic ligand defects through a competitive coordination strategy. In the solvothermal process, a certain amount of monocarboxylic acid molecules (thiophene-2-carboxylic acid) are added to react with metal ions (Zn 2+ ) can partially replace the original ligand (2,5-thiophenedicarboxylic acid) to produce a ligand defect.

[0070] (2) Changing the dosage of the modulator (thiophene-2-carboxylic acid, 2-chlorothiophene-5-carboxylic acid, 5-bromo-2-carboxythiophene) can affect the crystal orientation of MOFs or promote the formation of a specific crystal phase, thereby indirectly affecting the size and proportion of the pores. Adding ligands with halogen groups can act as Lewis acids to effectively adsorb LiPSs and reduce their solubility in the electrolyte, thereby inhibiting the shuttle effect.

[0071] (3) By carefully controlling the synthesis conditions, defects are introduced, which not only increases the specific surface area of ​​the material and creates more active sites, but also provides sufficient ion conduction channels to limit the diffusion of LiPSs. At the same time, it has good electrocatalytic ability, promotes the conversion kinetics of LiPSs under poor electrolyte conditions, and can improve the cycle stability of the battery.

[0072] The present invention is a method for modifying a diaphragm with defective structures in a metal organic framework. The defective crystal material is made into a slurry by a doctor blade method and coated on a PP diaphragm, and then assembled into a lithium sulfur battery for cycle testing. As shown in Table 1, the ratio of the modulator 2,5-thiophene dicarboxylic acid to thiophene-2-carboxylic acid is 7:3, which has the best battery performance at 0.1C.

[0073] Table 1 Effect of modulator ratio on battery performance (0.1C cycle)

[0074] 2,5-Thiophenedicarboxylic acid:Thiophene-2-carboxylic acid <![CDATA[Initial circle capacity (mAh·g -1 )]]> <![CDATA[Capacity after 50 cycles (mAh·g -1 )]]> 9:1 929 530.2 7:3 1531.7 653.4 5:5 933.6 590.7

[0075] The effect of the present invention is that an appropriate number of defects can be selected as catalytic active sites to promote the conversion reaction of polysulfides and improve the electrochemical activity of lithium-sulfur batteries. Defects can also change the electronic and ionic conductivity of MOFs. An appropriate amount of defects may accelerate the transmission of lithium ions by providing additional conduction paths, thereby improving the cycle stability of lithium-sulfur batteries. However, too many defects may increase the disorder of MOFs, hinder the migration of ions, and reduce battery performance; the present invention controls the number of defects by changing the amount of modulator used, thereby ensuring the efficiency of ion migration.

Claims

1. A method for modifying a diaphragm based on a metal organic framework defect structure, characterized in that: The method comprises the synthesis of a metal organic framework defect crystal material, mixing the defect metal organic framework material with a conductive agent and a binder, adding NMP, preparing a slurry and coating the slurry on a PP diaphragm to obtain a modified diaphragm.

2. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 1, characterized in that: The specific steps are as follows: Step 1: Weigh thiophene-2-carboxylic acid, 5-methyltetrazole and zinc nitrate hexahydrate, add them to a mixed solution of methanol and DMA, stir until the solution is uniform, then add 2,5-thiophenedicarboxylic acid, and then add tetramethylammonium hydroxide, put them into a reactor to react; then cool to room temperature, wash with N,N-dimethylacetamide, and dry to obtain a metal organic framework defect crystal material A; Step 2: Grind the defective crystal material A and the conductive agent obtained in step 1 evenly, then add a binder and N-methylpyrrolidone solution and stir to form a uniform slurry B; Step 3: Use a scraper to apply the slurry B in step 2 onto the PP diaphragm, and dry it in a vacuum drying oven to obtain a modified diaphragm C; Step 4: Use a punch to cut the modified diaphragm in step 3 into pieces to obtain a modified battery diaphragm D.

3. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 2, characterized in that: The thiophene-2-carboxylic acid in step 1 can be replaced by any one of 2-chlorothiophene-5-carboxylic acid and 5-bromo-2-carboxythiophene.

4. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 3, wherein the molar ratio of 2,5-thiophenedicarboxylic acid to thiophene-2-carboxylic acid is 9 to 1:1; The volume ratio of methanol to DMA in step 1 is 1:1, the temperature of the oven is set at 100° C. to 150° C., and the reaction time is between 36 h and 72 h.

5. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 2, characterized in that: In step 2, the defective crystal material A accounts for more than 50% of the conductive agent and the binder, and the stirring time is not less than 30 minutes.

6. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 2, characterized in that: In step 2, the conductive agent includes any one of Super P, graphene and Ketjen black; the binder includes any one of polyvinylidene fluoride, polytetrafluoroethylene and polyethylene oxide.

7. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 2, characterized in that: The modified diaphragm C described in step 3 is scraped to a thickness of 50 to 150 μm; the vacuum drying temperature is 50° C. to 70° C., and the time is not less than 12 hours.

8. The method for modifying a diaphragm based on a metal organic framework defect structure according to claim 2, characterized in that: The diameter of the diaphragm cut piece in step 4 is 19 mm.

9. A modified diaphragm based on a metal organic framework defect structure, characterized in that: The membrane is prepared by the method for modifying the membrane based on the defect structure of a metal organic framework as described in any one of claims 1 to 8.

10. A method for preparing a lithium-sulfur battery, using the modified diaphragm based on metal organic framework defect structure according to claim 9, characterized in that: The modified separator D, S@CNT composite positive electrode material, metal lithium sheet negative electrode material spring and gasket were assembled into a lithium-sulfur battery in a glove box, and the battery cycle, rate, impedance and CV curve were tested at different currents; The different currents include 0.1C, 0.2C, 0.5C, 1C, and 2C; the parameter frequency tested when testing electrochemical impedance is 0.01-1000000 Hz, the cyclic voltammetry test voltage is 1.6V-2.8V, and the scan rate is 0.0001V / s-0.0005V / s.

Citation Information

Patent Citations

  • Preparation method of composite diaphragm of lithium-sulphur battery

    CN104393220A

  • Preparation method of novel lithium-sulfur battery diaphragm material

    CN110611068A

  • Lithium-sulfur and sodium-sulfur battery cathodes

    CN112352334A

  • Preparation method of Zn-based dual-MOF modified diaphragm for lithium-sulfur battery as well as product and application of Zn-based dual-MOF modified diaphragm

    CN115810865A

  • Separator for nonaqueous electrolyte secondary battery, method of manufacturing the same, and nonaqueous electrolyte secondary battery

    JP2013157266A

Cited By

  • Preparation method of multi-acid-group covalent organic framework modified diaphragm, modified diaphragm and lithium-sulfur battery

    CN119764744A