ZnO nano piezoelectric photocatalyst as well as preparation method and application thereof
Hexagonal sheet ZnO nano-piezoelectric photocatalyst was prepared by sol-gel method and solvothermal method, and the crystal surface exposure ratio was adjusted. The piezoelectric effect and crystal surface effect were used to solve the problem of low performance of existing ZnO nanorod catalysts, and the realization of Highly efficient photocatalytic properties and rapid organic degradation.
Patent Information
- Application Number
- CN202411447078.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ZnO nanorod catalysts are prone to block the pores in actual use, their performance is reduced and they are prone to fall off. The prior art cannot effectively promote the separation and transmission of photogenerated carriers, resulting in limited photocatalytic performance.
Hexagonal sheet ZnO nano-piezoelectric photocatalysts of different thicknesses are prepared by sol-gel method and solvothermal method, and the crystal surface exposure ratio is adjusted, and the piezoelectric effect and crystal surface effect are used to promote unidirectional transmission of photogenerated carriers, reducing the recombination probability. Improve carrier transmission efficiency.
It significantly improves the carrier transfer efficiency of ZnO photocatalysts, reduces photogenerated carrier recombination, generates a large number of superoxide radicals and hydroxyl radicals, enhances the degradation ability of organic matter in water, and quickly removes organic dyes and antibiotics in water.
Smart Images

Figure CN118988282A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of piezoelectric photocatalysts, and in particular to a ZnO nanometer piezoelectric photocatalyst and a preparation method and application thereof. Background Art
[0002] In recent years, various environmental pollutants such as synthetic dyes, phenolic compounds, organophosphates and their derivatives, and antibiotics have become a major threat to human health. In order to solve this problem, people have widely explored a variety of treatment technologies such as photocatalytic degradation, adsorption, biological treatment, and flocculation precipitation to eliminate organic pollutants in water. Among these methods, semiconductor photocatalysis is considered to be a promising advanced oxidation process (AOPs) with superior stability, high efficiency, and green sustainability.
[0003] However, semiconductor photocatalysis still faces some great challenges, for example, the migration efficiency of existing photocatalysts is low, and photogenerated carriers are very easy to recombine, resulting in poor redox performance. Therefore, it is worthwhile to find various methods to improve the performance of photocatalysts.
[0004] In recent years, the concept of piezoelectric photocatalysis has been proposed and has made great progress. When piezoelectric materials are subjected to stress, the piezoelectric potential generated by the formation of non-zero dipole moment due to the change in crystal structure is conducive to promoting the separation and transfer of photogenerated charges, and has become a key way to improve the efficiency of photocatalysis. The composite material composed of piezoelectric materials and photocatalysts is placed in polluted water. Under the synergistic effect of mechanical energy such as ultrasound, water flow, and waves and light, the piezoelectric potential can continuously promote the separation and transfer of free charges generated on the surface of the photocatalyst, and then react with water molecules or oxygen dissolved in water to generate ·OH, ·O 2 - Since ZnO has both piezoelectric and semiconductor properties, the piezoelectric potential generated in the crystal can significantly affect the carrier transport in the interface / junction region, and only one material is needed to achieve piezoelectric photocatalysis.
[0005] Benefiting from the anisotropy of crystals, nanocatalysts with multiple crystal faces usually exhibit crystal face-dependent physical and chemical properties (such as geometric structure, surface electronic structure, surface built-in electric field and redox active sites, etc.), resulting in different energy levels of each crystal face, so that electrons and holes can be transmitted unidirectionally to different crystal faces, improving their photogenerated carrier transmission efficiency. Crystal face regulation strategies can expose crystal faces with high catalytic activity on the catalyst surface.
[0006] Chinese patent CN117398988A discloses a method for improving the surface photovoltage of ZnO. In this invention, fullerene (C60 and C 70 ), can affect the crystal structure and optical properties of ZnO, and enhance the photocatalytic performance through the interaction between ZnO and fullerene. At the same time, this invention is simple to operate, green and environmentally friendly and easy to implement. This invention improves the generation efficiency of photogenerated carriers, but has no obvious promoting effect on the separation and transmission of photogenerated carriers, and the performance improvement is limited.
[0007] Chinese patent CN111921517A discloses a method for preparing a foam ceramic-based ZnO nanorod array, and the resulting catalyst has excellent photocatalytic water splitting activity and stability. The ZnO nanorod array is directly grown on the foam ceramic substrate, and the interconnected pore structure of the foam ceramic is utilized, and the natural micro-energy (fluid mechanical energy) in the catalytic environment is used to generate eddy currents in the foam ceramic pores, so that the ZnO array is repeatedly deformed, which can effectively promote the separation of photogenerated charges and reduce the recombination of photogenerated electron-hole pairs, thereby improving the photocatalytic performance. However, the above patent preparation is based on ZrO 2 ZnO nanorods grown on ceramics are very likely to block the pores in actual use, greatly reducing the overall performance. At the same time, ZnO nanorods are very easy to fall off, which also limits their use. Summary of the invention
[0008] In view of the defects or improvement needs of the prior art, the purpose of the present invention is to provide a ZnO nano-piezoelectric photocatalyst and a preparation method and application thereof, so as to effectively solve the problems existing in the prior art.
[0009] In order to achieve the above purpose or other purposes, the present invention provides a ZnO nano-piezoelectric photocatalyst and a preparation method and application thereof, which are achieved through the following technical solutions.
[0010] A method for preparing a ZnO nano-piezoelectric photocatalyst comprises the following steps: (1) heating the zinc source to remove crystal water to obtain an anhydrous zinc source, which is then sealed and stored; (2) Add anhydrous zinc source to the solvent, gradually raise the temperature while stirring until the zinc source is completely dissolved, continue to keep the temperature until a white precipitate is produced, and continue to stir after the white precipitate is produced to complete the reaction; (3) washing the white precipitate obtained in step (2) with anhydrous ethanol and drying it to obtain a white complex precursor; (4) Take the white complex precursor obtained in step (3), add the mixed solvent, and stir until it is uniformly dissolved; (5) subjecting the solution obtained in step (4) to a hydrothermal reaction; (6) After the reaction is completed, the white precipitate produced by the reaction is taken out, washed and dried to obtain ZnO with polycrystalline faces exposed in different crystal face exposure ratios, which is the ZnO nanopiezoelectric photocatalyst.
[0011] Furthermore, the zinc source is selected from one or more of zinc chloride, zinc acetate dihydrate, zinc hydroxide, zinc sulfate heptahydrate, and zinc nitrate hexahydrate.
[0012] Furthermore, in step (2), the solvent is selected from one or more of propylene glycol (glycerol), isopropanol, n-butanol, ethylene glycol, ethyl acetate, and diethylene glycol butyl ether.
[0013] Furthermore, the heating temperature in step (1) is 80°C to 200°C.
[0014] Furthermore, in step (2), the mass volume ratio of the anhydrous zinc source to the solvent is 1:(1-100), that is, 1 g of anhydrous zinc source is added to a solvent volume of 1-100 mL.
[0015] Furthermore, in step (2), the reaction is continued to be stirred for 10 to 60 min after a white precipitate is generated.
[0016] Furthermore, in step (3), the drying temperature is 40-150° C., and the drying time is 6 h-72 h.
[0017] Furthermore, in step (4), the mass volume ratio of the white complex precursor to the mixed solvent is 1:(1-100), that is, 1 g of the white complex precursor is added to a volume of 1-100 mL of the mixed solvent.
[0018] Furthermore, in step (4), the mixed solvent is selected from a mixed solvent of water and alcohol. Preferably, the volume ratio of water to alcohol in the mixed solvent is 1:20 to 20:1. More preferably, the mixed solvent of water and alcohol is selected from a mixed solvent of water and ethanol, a mixed solvent of water and isopropanol, or a mixed solvent of water and n-butanol.
[0019] Furthermore, in step (5), the hydrothermal reaction time is 2 h to 24 h.
[0020] Furthermore, in step (5), the hydrothermal reaction temperature is 80°C to 200°C.
[0021] Furthermore, in step (6), deionized water and ethanol are used for washing respectively, and after washing, the mixture is dried at 40°C to 120°C.
[0022] The present invention also provides a ZnO nano-piezoelectric photocatalyst prepared by the above method. The obtained ZnO nano-piezoelectric photocatalyst is in the shape of a hexagonal sheet. The ZnO nano-piezoelectric photocatalyst prepared by the present invention has two different exposed crystal faces, and a crystal face junction can be formed between the two crystal faces, so that electrons and holes are transmitted to the two crystal faces respectively, which improves the separation and transmission efficiency of electrons and holes, reduces the probability of electron and hole recombination inside and on the surface of the material, and improves the performance of piezoelectric photocatalysis. At the same time, the crystal face exposure ratio of the ZnO nano-piezoelectric photocatalyst in the present invention can be adjusted by adjusting the reaction parameters.
[0023] The third aspect of the present invention provides an application of a ZnO nano-piezoelectric photocatalyst in the field of piezoelectric photocatalysts.
[0024] The present invention provides a ZnO nano-piezoelectric photocatalyst and a preparation method thereof. In the present invention, a sol-gel method and a solvothermal method are used to prepare ZnO hexagonal sheets of different thicknesses by adjusting experimental parameters. The ZnO nano-piezoelectric photocatalyst with adjustable crystal face exposure ratio prepared by the present invention greatly improves the carrier transmission efficiency of the ZnO photocatalyst through the synergistic effect of crystal face engineering and piezoelectric effect. The crystal face effect and the external piezoelectric field enable photogenerated electrons and holes to be transmitted unidirectionally, significantly reducing the recombination of photogenerated carriers, promoting the transfer of photogenerated carriers, and generating a large number of superoxide radicals, hydroxyl radicals and holes, thereby giving it a strong degradation ability for organic matter in water, thereby quickly removing organic dyes and antibiotics in water. The free radicals with high oxidation potential generated by the system can also treat other difficult-to-degrade organic matter in water or produce hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The XRD diagrams of the catalysts prepared in Examples 1-5 of the present invention and the comparative example.
[0026] Figure 2 The SEM images are of the morphologies of the products obtained in Examples 1-5 of the present invention and the comparative example respectively.
[0027] Figure 3 The performance comparison of the products prepared in Example 1 of the present invention and the comparative example in the piezoelectric photocatalytic degradation of tetracycline hydrochloride (TC) is shown.
[0028] Figure 4 This is a performance comparison chart of the products prepared in Examples 1-5 of the present invention for the piezoelectric photocatalytic degradation of tetracycline hydrochloride (TC). DETAILED DESCRIPTION
[0029] The following describes the implementation of the present invention through specific embodiments, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific implementations, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0030] It should be noted that, in the absence of conflict, the features in the following examples and embodiments can be combined with each other. It should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments rather than to limit the scope of the present invention. The test methods in the following examples that do not specify specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers.
[0031] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention. Example
[0032] The preparation of the hexagonal ZnO nano-piezoelectric photocatalyst with adjustable crystal surface exposure ratio in this embodiment includes the following steps: Step 1: 20 g of zinc acetate dihydrate (Zn(CH 3 COO 2 ·2H 2 O) putting it into an oven and heating it at 100°C to remove the crystal water to obtain anhydrous zinc acetate, which is then sealed and stored; Step 2: Take 8 g of anhydrous zinc acetate (Zn(CH 3 COO 2 ) was added into 60 mL of ethylene glycol, the temperature was raised while stirring, and stirring was continued for 60 min after a white precipitate was produced; Step 3, washing the white precipitate obtained in step 2 with anhydrous ethanol for 3-5 times, drying at 80° C. overnight (i.e., drying for 12 hours) to obtain a white precipitate, which is a precursor; Step 4: Take 3 g of the white precipitate precursor, add a total of 70 mL of a mixed solvent of water and ethanol in a ratio of 1:1, and stir until it is evenly dissolved.
[0033] Step 5, transfer the solution into a polytetrafluoroethylene reactor, place it in an oven, and perform a hydrothermal reaction at 100° C. for 9 h; Step 6, taking out the white precipitate produced in the polytetrafluoroethylene reactor, washing the precipitate with deionized water and ethanol for 3-5 times respectively, removing impurities, and drying at 120° C. overnight to obtain the final product; Example
[0034] The preparation of the hexagonal ZnO nano-piezoelectric photocatalyst with adjustable crystal surface exposure ratio in this embodiment includes the following steps: Step 1: 20 g of zinc acetate dihydrate (Zn(CH 3 COO 2 ·2H 2 O) placing in an oven and heating at 120°C to remove crystal water to obtain anhydrous zinc acetate, which is then sealed and stored; Step 2: Take 8 g of anhydrous zinc acetate (Zn(CH 3 COO 2 ) was added into 80 mL of propylene glycol, the temperature was raised while stirring, and stirring was continued for 60 min after a white precipitate was produced; Step 3, washing the white precipitate obtained in step 2 with anhydrous ethanol for 3-5 times, drying at 80° C. overnight (i.e., drying for 12 hours) to obtain a white precipitate as a precursor; Step 4: Take 5 g of the white precipitate precursor, add a total of 70 mL of a mixed solvent of water and isopropanol in a ratio of 1:3, and stir until it is evenly dissolved.
[0035] Step 5, transfer the solution into a polytetrafluoroethylene reactor, place it in an oven, and perform a hydrothermal reaction at 100° C. for 9 h; Step 6: Take out the white precipitate produced in the polytetrafluoroethylene reactor, wash the precipitate with deionized water and ethanol for 3-5 times respectively, remove impurities, and dry it at 100° C. overnight to obtain the final product. Example
[0036] The preparation of the hexagonal ZnO nano-piezoelectric photocatalyst with adjustable crystal surface exposure ratio in this embodiment includes the following steps: Step 1: 20 g of zinc acetate dihydrate (Zn(CH 3 COO 2 ·2H 2 O) putting it into an oven and heating it at 200°C to remove the crystal water to obtain anhydrous zinc acetate, which is then sealed and stored; Step 2: Take 8 g of anhydrous zinc acetate (Zn(CH 3 COO 2 ) was added into 80 mL of propylene glycol, the temperature was raised while stirring, and stirring was continued for 30 min after a white precipitate was produced; Step 3, washing the white precipitate obtained in step 2 with anhydrous ethanol for 3-5 times, drying at 80° C. overnight (i.e., drying for 12 hours) to obtain a white precipitate as a precursor; Step 4: Take 8 g of the white precipitate precursor, add a total of 80 mL of a mixed solution of water and isopropanol in a ratio of 3:1, and stir until the solution is uniform.
[0037] Step 5, transfer the solution into a polytetrafluoroethylene reactor, place it in an oven, and perform a hydrothermal reaction at 100° C. for 9 h; Step 6: Take out the white precipitate produced in the polytetrafluoroethylene reactor, wash the precipitate with deionized water and ethanol for 3-5 times respectively, remove impurities, and dry at 50° C. overnight to obtain the final product. Example
[0038] The preparation of the hexagonal ZnO nano-piezoelectric photocatalyst with adjustable crystal surface exposure ratio in this embodiment includes the following steps: Step 1: 20 g of zinc nitrate hexahydrate (Zn(NO 3 ) 2 6H 2 O) putting it into an oven and heating it at 100°C to remove the crystal water to obtain anhydrous zinc acetate, which is then sealed and stored; Step 2: Take 8 g of anhydrous zinc nitrate (Zn(NO 3 ) 2 ) was added into 60 mL of n-butanol, the temperature was raised while stirring, and stirring was continued for 10 min after a white precipitate was produced; Step 3, washing the white precipitate obtained in step 2 with anhydrous ethanol for 3-5 times, and drying at 80°C overnight (i.e., drying for 12 hours) to obtain a white precipitate as a precursor; Step 4: Take 1 g of the precursor, add 60 mL of a mixed solution of water and ethanol in a ratio of 1:1, and stir until it is evenly dissolved.
[0039] Step 5, transfer the solution into a polytetrafluoroethylene reactor, place it in an oven, and perform a hydrothermal reaction at 150° C. for 6 h; Step 6: Take out the white precipitate produced in the polytetrafluoroethylene reactor, wash the precipitate with deionized water and ethanol for 3-5 times respectively, remove impurities, and dry it at 80° C. overnight to obtain the final product. Example
[0040] The preparation of the hexagonal ZnO nano-piezoelectric photocatalyst with adjustable crystal surface exposure ratio in this embodiment includes the following steps: Step 1: Take 8 g zinc chloride (ZnCl 2) was added into 80 mL of ethylene glycol, the temperature was raised while stirring, and stirring was continued for 60 min after a white precipitate was produced; Step 2: Wash the white precipitate obtained in step 1 with anhydrous ethanol for 3-5 times, and dry it at 80°C overnight (i.e., dry it for 12 hours) as a precursor; Step 3: Take 4 g of the precursor, add 60 mL of a mixed solution of water and ethanol in a ratio of 1:1, and stir until the solution is uniform.
[0041] Step 4, transfer the solution into a polytetrafluoroethylene reactor, place it in an oven, and perform a hydrothermal reaction at 120° C. for 10 h; Step 5: Take out the white precipitate produced in the polytetrafluoroethylene reactor, wash the precipitate with deionized water and ethanol for 3-5 times respectively, remove impurities, and dry it at 40° C. overnight to obtain the final product. Example
[0042] The specific preparation method of this embodiment is the same as that of Example 1, except that in step 2, 8 g of anhydrous zinc acetate (Zn(CH 3 COO 2 ) is added to 800 mL of ethylene glycol; Step 4, take 3 g of the white precipitate precursor and add a total of 300 mL of a mixed solvent of water and ethanol in a ratio of 1:1. Example
[0043] The specific preparation method of this embodiment is the same as that of Example 1, except that in step 2, 8 g of anhydrous zinc acetate (Zn(CH 3 COO 2 ) is added to 8 mL of ethylene glycol; Step 4, take 3 g of the white precipitate precursor and add a total of 3 mL of a mixed solvent of water and ethanol in a ratio of 1:1.
[0044] Step 1: 2 g of zinc acetate dihydrate (Zn(CH 3 COO 2 ·2H 2 O) was dissolved in 20 mL of water and stirred until completely dissolved as solution A; Step 2: Dissolve 2 g of ammonium carbonate in 20 mL of water and stir until completely dissolved, as solution B. Step 3: Slowly drop solutions A and B into 100 mL of vigorously stirred polyethylene glycol (PEG) aqueous solution and filter to obtain a white precipitate.
[0045] Step 4: Wash the white precipitate obtained in step 3 with water and ethanol three times respectively, and dry it in an oven at 100° C. overnight.
[0046] Step 5: Take 3 g of the dried white precipitate and add it to a ball mill, and ball mill it at 1000 rpm for 1 h.
[0047] Step 6: The sample was transferred into a crucible and calcined at 450° C. for 2 h in an air atmosphere to obtain the final product.
[0048] The products obtained in Examples 1-5 and the comparative example were characterized by X-ray diffraction (XRD) instrument (instrument model: Smart-Lab SE). The results are as follows: Figure 1 As shown in the figure, it can be seen that its characteristic peaks are basically consistent with the ZnO standard card PDF#76-0704, proving that its composition is ZnO.
[0049] 2. The products obtained in Examples 1-5 and Comparative Example were photographed using a scanning electron microscope (SEM). The results are as follows: Figure 2 As shown, by comparing the morphology of the products obtained in Examples 1-5 with those in the comparative example, it can be found that the products in Examples 1-5 of the present invention are all hexagonal flake ZnO, but their thickness and the ratio of crystal surface exposure are different, while the comparative example products appear as irregular spherical nanoparticles.
[0050] 3. The products obtained in Example 1 and the comparative example were subjected to a comparative test on the performance of piezoelectric photocatalytic degradation of tetracycline hydrochloride (TC) using an ultraviolet-visible-near infrared spectrophotometer (instrument model: UV-3600 Plus). Figure 3 As shown, compared with the sample of the comparative example, the hexagonal flaky ZnO nanoparticles with exposed polycrystalline faces formed in Example 1 of the present application have higher photocatalytic activity.
[0051] 4. Compare the piezoelectric photocatalytic degradation performance of tetracycline hydrochloride of the products obtained in Examples 1-5. Figure 4 As shown, compared with the samples of Experimental Examples 2 and 3, the thickness of the hexagonal flaky ZnO nanoparticles formed in Example 1 of the present application is the most suitable, and the ratio of the two crystal planes is the closest, so its photocatalytic activity is higher.
[0052] The sol-gel + hydrothermal preparation process of the hexagonal plate-shaped ZnO nano piezoelectric photocatalyst with adjustable crystal face exposure ratio provided by the present invention prepares a hexagonal plate-shaped ZnO nano piezoelectric photocatalyst with polycrystalline face exposure that can adjust the crystal face exposure ratio. In addition, the application of the hexagonal plate-shaped ZnO nano piezoelectric photocatalyst with polycrystalline face exposure to the piezoelectric photocatalytic system can efficiently generate free radicals, thereby quickly removing organic dyes and antibiotics in water. Of course, the free radicals with high oxidation potential generated by the system can also treat other difficult-to-degrade organic matter in water.
[0053] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a ZnO nanopiezoelectric photocatalyst, characterized in that: The following steps are involved: (1) heating the zinc source to remove crystal water to obtain an anhydrous zinc source, which is then sealed and stored; (2) Add anhydrous zinc source to the solvent, gradually raise the temperature while stirring until the zinc source is completely dissolved, continue to keep the temperature until a white precipitate is produced, and continue to stir after the white precipitate is produced to complete the reaction; (3) washing the white precipitate obtained in step (2) with anhydrous ethanol and drying it to obtain a white complex precursor; (4) Take the white complex precursor obtained in step (3), add the mixed solvent, and stir until it is uniformly dissolved; (5) subjecting the solution obtained in step (4) to a hydrothermal reaction; (6) After the reaction is completed, the white precipitate produced by the reaction is taken out, washed and dried to obtain ZnO with polycrystalline faces exposed in different crystal face exposure ratios, which is the ZnO nanopiezoelectric photocatalyst.
2. The preparation method according to claim 1, characterized in that Include one or more of the following technical features: The zinc source is selected from one or more of zinc chloride, zinc acetate dihydrate, zinc hydroxide, zinc sulfate heptahydrate, and zinc nitrate hexahydrate; In step (2), the solvent is selected from one or more of glycerol, isopropanol, n-butanol, ethylene glycol, ethyl acetate, and diethylene glycol butyl ether; The mixed solvent in step (4) is selected from a mixed solvent of water and alcohol.
3. The preparation method according to claim 1, characterized in that: In step (2), the mass volume ratio of the anhydrous zinc source to the solvent is 1:(1-100).
4. The preparation method according to claim 1, characterized in that: In step (4), the mass volume ratio of the white complex precursor to the mixed solvent is 1:(1-100).
5. The preparation method according to claim 1, characterized in that: In step (5), the hydrothermal reaction time is 2 h to 24 h.
6. The preparation method according to claim 1, characterized in that: In step (5), the hydrothermal reaction temperature is 80°C to 200°C.
7. The ZnO nanopiezoelectric photocatalyst prepared by the preparation method according to any one of claims 1 to 6.
8. Application of the ZnO nano-piezoelectric photocatalyst prepared by the preparation method according to any one of claims 1 to 6 in the field of piezoelectric photocatalysts.
Citation Information
Patent Citations
Preparation method of flaky nanometer zinc oxide powder
CN101767813A
Method for preparing nano-zinc oxide used as photocatalyst
CN104307501A
Preparation method of hexagonal prism zinc oxide
CN109987623A
AU2020102586A4
Cited By
Method for directionally regulating and controlling morphology of ZnO / CuO piezoelectric catalyst based on betulinic acid self-assembly and piezoelectric application of ZnO / CuO piezoelectric catalyst
CN120900718A