Flash welding construction method for all steel rail joints of turnout

By pre-laying extended guide rails inside the turnout and combining them with precision rail sawing technology, the welding problems caused by the narrow space inside the turnout and rail wear were solved, achieving high-quality flash welding of all rail joints of the turnout, thus improving the safety and operational reliability of the turnout.

CN118989540APending Publication Date: 2024-11-22中铁十七局集团深圳建设有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411240066.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The welding space at the location of the rail joints inside the turnout is extremely narrow, making it impossible to directly use flash welding technology. Furthermore, rail wear during the welding process makes it difficult to adjust the changes in the turnout's structural dimensions.

Method used

By using extended guide rails, the welding loss is concentrated on the extended guide rails through pre-laying and adjusting the internal structural dimensions of the turnout. Combined with precision rail sawing technology, this ensures that the welded turnout meets the acceptance standards.

Benefits of technology

High-quality flash welding of all rail joints of the turnout was achieved, reducing rail breakage rate and maintenance costs, and improving the safety and operational reliability of the turnout.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989540A_ABST
    Figure CN118989540A_ABST
Patent Text Reader

Abstract

The invention particularly relates to a flash welding construction method for all steel rail joints of a turnout. The method comprises the following steps: pre-paving the turnout, and adjusting the structural size; marking the relative position of the switch rail point and the stock rail as a control reference; the curved switch rail and the curved upper strand guide rail are detached, and a lengthened straight upper strand guide rail is laid for welding; welding and re-laying the dismantled curved switch rail and the lengthened curved upper strand guide rail; the straight switch rail and the straight lower strand guide rail are detached, and the lengthened curved lower strand guide rail is laid for welding; welding the detached straight switch rail and the lengthened straight lower strand guide rail and re-laying the straight switch rail and the lengthened straight lower strand guide rail; the excess of the lengthened guide rail is sawed, and then the lengthened guide rail is welded to the frog head; after the excess of the guide rail is lengthened, sawing the guide rail, and then welding the guide rail with a straight upper rail and a curved lower rail of the frog part, and then performing diffusion locking; sequentially completing the welding of the turnout and the adjacent track, and locking the steel rails at the two ends of the turnout after the construction is finished; and the quality of the steel rail joint in the turnout is comprehensively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of railway seamless turnout welding construction, in particular to a flash welding construction method for all rail joints of a turnout. Background Art

[0002] Railway transportation is an important mode of transportation in my country. With the rapid development of social economy, people have higher and higher requirements for line laying. As one of the weak links in the quality of railway construction, the quality of the welding joints of turnouts directly affects the safety of locomotive operation. At present, thermite welding (the welding principle is to fix a shaping mold such as a crucible at the rail joint, put thermite flux in the crucible and heat it, so that it undergoes an exothermic oxidation-reduction reaction and releases a large amount of heat. The generated molten iron welds the two rails together, which can be completed by manual cooperation with simple machines) is the main method for welding turnout joints on railway seamless lines at home and abroad due to its advantages such as simple equipment, convenient operation, and no shortening of the rails. However, the weld of thermite welding joint forms a casting structure, and the comprehensive mechanical properties of the weld are greatly reduced compared with the parent material, so that the weld strength and the service life of the rail are often only about one-third to three-quarters of the parent material, resulting in frequent replacement of turnouts and extremely high maintenance costs. Compared with flash welding, thermite welding has poor welding quality, low joint strength, high frequency of flaw detection and rail breakage rate. According to statistics, the rail breakage rate of thermite welding head is about 10 times that of flash welding head, which brings greater hidden dangers to railway driving safety and operation management, and is the difficulty and focus of maintenance.

[0003] Rail flash welding is completed by a mobile flash welding machine, which has a high degree of automation, stable process and excellent welding quality. Its welded joint is a dense forging structure, and its mechanical properties are close to those of the rail parent material. It is currently the most practical, highest welding precision and best welding quality welding method for rail welding, and is also the main method for welding long rails in railway sections. There is no essential difference between the welding of turnout rail joints and the welding of long rail joints in sections. The traditional thermite welding process has gradually become unable to meet the locomotive's increasingly high quality requirements for turnout rail welds. Using welding processes with better welding quality to replace thermite welding has become a development trend for turnout welding. However, since the welding space at some rail joints inside the turnout is extremely small and limited, ordinary welding machines cannot perform direct welding, and the rail joints will produce 3cm to 4cm of loss and a certain displacement during the flash welding upsetting process, which makes it extremely difficult to adjust the structure size of the turnout. As a result, the flash welding process cannot be directly applied to the welding of the internal joints of the turnout. On the other hand, there is currently a surplus of mobile flash welding equipment for rails on the mainline of the railway. Compared with the turnouts and branch line rail joints, which have a larger number of rail joints on the mainline of the railway, there is a situation where there is no equipment available for welding.

[0004] Therefore, it is necessary to invent a kind of flash welding construction method of all rail joints of turnout to solve the problems referred to above. Summary of the invention

[0005] In order to solve the technical problems that flash welding is accompanied by rail loss, resulting in changes in the size of the turnout structure and difficulty in adjusting it, and the technical problem that the welding space at the location of some rail joints inside the turnout is extremely narrow and limited and flash welding of the turnout cannot be achieved, the present invention provides a flash welding construction method for all rail joints of the turnout.

[0006] The present invention is achieved by adopting the following technical solutions: A flash welding construction method for all rail joints of a turnout, comprising a turnout, wherein the turnout comprises a base rail, a point rail, an upper rail, a lower rail, a rudder rail and a rudder, wherein the base rail comprises a straight base rail and a curved base rail, the point rail comprises a straight point rail and a curved point rail, the upper rail comprises a straight upper rail and a curved upper rail, the lower rail comprises a straight lower rail and a curved lower rail, and the rudder rail comprises a rudder straight upper rail and a rudder curved lower rail; It also includes an extended guide rail, which includes an extended straight upper guide rail, an extended curved upper guide rail, an extended straight lower guide rail and an extended curved lower guide rail of the same length, and the length of the extended guide rail = (theoretical top forging burnout amount of rail flash welding + actual welding theoretical error value + joint rail gap value + surplus amount) × 2; This method is implemented by the following steps: S1: Lay the rail components of the turnout, install the fasteners, and then adjust the internal structure dimensions of the turnout to meet the acceptance standards; S2: Mark the corresponding position of the tip of the pointed rail on the base rail as the control reference; S3: Remove the curved point rail and the curved upper strand guide rail, remove the straight upper strand guide rail and replace it with an extended straight upper strand guide rail, take the straight basic rail as the static end, complete the welding between it and the extended straight upper strand guide rail, and then install the fasteners of the extended straight upper strand guide rail; S4: weld the removed curved point rail and the extended curved upper rail outside the turnout, and then re-lay the curved point rail and the extended curved upper rail; S5: Remove the straight point rail and the straight lower rail, remove the curved lower rail and replace it with an extended curved lower rail, take the curved basic rail as the static end, complete the welding between it and the extended curved lower rail, and then install the fasteners of the extended curved lower rail; S6: weld the removed straight point rail and the extended straight down rail outside the turnout, and then re-lay the straight point rail and the extended straight down rail; S7: After calculating the excess length of the extended guide rail, saw the rail and then weld it to the switch head; S8: after calculating the excess length of the extended guide rail, sawing the rail is performed, and then welding the rail with the upper rail of the turnout part and the lower rail of the turnout part is performed to release and lock the turnout; S9: After the release is completed, the turnout end is taken as the static end, and the welding of the turnout and its adjacent track is completed in sequence. After the construction is completed, the rails at both ends of the turnout are locked. At this time, the flash welding construction of the turnout rail joint is completed.

[0007] The present invention completes the pre-laying of the turnout in advance and adjusts the structural dimensions in the turnout in place according to the acceptance standard, and takes the position of the turnout assembly in this state as a control reference after the subsequent flash welding is completed; the principle of taking the turnout and the base rail as static ends in the intermediate and subsequent construction is that the positions of the turnout and the base rail are always kept unchanged during the welding process; the position of the straight and curved point rails is controlled by marking the relative position of the point rail and the base rail in the pre-laying state as a control reference, and the control reference is combined with the theoretical top forging burnt amount of the rail flash welding as the reserved loss amount, assisted by accurate rail sawing and welding, so that the allowable error requirement of the turnout size in the acceptance standard can be met.

[0008] A construction method for flash welding all rail joints of a turnout, wherein in step S4 and step S6, spacer irons and stoppers are temporarily removed during the laying process.

[0009] A construction method for flash welding all rail joints of a turnout, step S7 is implemented by the following steps: S7.1: Measure the misalignment between the two rail tips and the adjacent control datums respectively, reserve the theoretical top forging burnout amount of the rail flash welding at the tail end of the extended curved upper rail and the extended straight lower rail, and saw off the excess rail at the head end of both rails. The length of the excess rail is the misalignment minus the theoretical top forging burnout amount of the rail flash welding, and ensure that the relative distance between the two rail tips is not more than 5 mm; S7.2: With the switch as the static end, complete the welding of the extended curved upper rail, the extended straight lower rail and the switch head in sequence, and resume the installation of fasteners, spacers and limiters.

[0010] A construction method for flash welding all rail joints of a turnout, step S8 is implemented by the following steps: S8.1: Loosen the fasteners of the upper rail and the lower rail of the turnout in sequence, saw off the excess rails at the tail of the extended upper rail and the extended lower rail, and reserve the theoretical top forging burnout amount of the rail flash welding as the loss of the rail welding. The excess rail length is the actual welding theoretical error value plus the surplus amount; S8.2: With the extended straight upper rail and the extended curved lower rail as the static ends, complete the welding of the extended straight upper rail and the straight upper rail of the switch section, and the extended curved lower rail and the curved lower rail of the switch section in sequence, and restore the fasteners; S8.3: Release the lock of the turnout within the locking rail temperature range.

[0011] A construction method for flash welding all rail joints of a turnout. AT rails are used at some welding points of the turnout. When welding joints near the AT rails, the guide electrode of the flash welding is replaced by a guide electrode whose contact surface matches the waist surface of the AT rail.

[0012] The present invention combines the gradual change law of the waist thickness and cross-sectional height of the AT rail, redesigns and processes the clamping surface shape of a set of detachable clamping guide electrodes of a flash welding machine, and can perfectly fit with the surface of the clamping part of the AT rail with varying waist size and cross-sectional height, thereby ensuring the normal guiding and auxiliary clamping functions of the AT rail, solving the problem that general welding machines cannot effectively clamp and weld variable-section rails, and realizing flash welding of AT rail joints.

[0013] The present invention achieves the purpose of offsetting the loss of flash welding rails by concentrating the loss of turnout flash welding joints on four extended guide rails in advance and assisting with precise rail sawing, thereby solving the problem of changes in turnout component length and structural dimensions caused by rail loss during flash welding construction; at the same time, the four extended guide rails are standard long rails, and there is no need to adjust any turnout component dimensions through the turnout manufacturer, and long rails of the same model and type can be easily sawed on the long rails according to the design length by taking the extension amount into consideration.

[0014] The present invention can solve the problem of insufficient welding space for rail joints by adjusting the laying and welding construction organization.

[0015] The present invention achieves a technical breakthrough from thermite welding to flash welding of all rail joints of the turnout by adjusting the construction organization sequence of laying and welding and lengthening some guide rails, thereby comprehensively improving the quality of the rail joints inside the turnout, and can greatly reduce the rail breakage rate, safety risks, and maintenance workload of the rail joints inside the turnout after the line is opened for operation. The present invention has strong applicability and great significance for promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the structure of the present invention; Figure 2 is a schematic diagram of step S3 in the present invention; Figure 3 is a schematic diagram of step S4 in the present invention; Figure 4 is a schematic diagram of step S5 in the present invention; Figure 5 It is a schematic diagram of step S6 in the present invention. DETAILED DESCRIPTION

[0017] A flash welding construction method for all rail joints of a turnout, comprising a turnout, wherein the turnout comprises a base rail, a point rail, an upper rail, a lower rail, a rudder rail and a rudder, wherein the base rail comprises a straight base rail and a curved base rail, the point rail comprises a straight point rail and a curved point rail, the upper rail comprises a straight upper rail and a curved upper rail, the lower rail comprises a straight lower rail and a curved lower rail, and the rudder rail comprises a rudder straight upper rail and a rudder curved lower rail; It also includes an extended guide rail, which includes an extended straight upper guide rail, an extended curved upper guide rail, an extended straight lower guide rail and an extended curved lower guide rail of the same length, and the length of the extended guide rail = (theoretical top forging burnout amount of rail flash welding + actual welding theoretical error value + joint rail gap value + surplus amount) × 2; This method is implemented by the following steps: S1: Lay the rail components of the turnout, install the fasteners, and then adjust the internal structure dimensions of the turnout to meet the acceptance standards; S2: Mark the corresponding position of the tip of the pointed rail on the base rail as the control reference; S3: Remove the curved point rail and the curved upper strand guide rail, remove the straight upper strand guide rail and replace it with an extended straight upper strand guide rail, take the straight basic rail as the static end, complete the welding between it and the extended straight upper strand guide rail, and then install the fasteners of the extended straight upper strand guide rail; S4: weld the removed curved point rail and the extended curved upper rail outside the turnout, and then re-lay the curved point rail and the extended curved upper rail; S5: Remove the straight point rail and the straight lower rail, remove the curved lower rail and replace it with an extended curved lower rail, take the curved basic rail as the static end, complete the welding between it and the extended curved lower rail, and then install the fasteners of the extended curved lower rail; S6: weld the removed straight point rail and the extended straight down rail outside the turnout, and then re-lay the straight point rail and the extended straight down rail; S7: After calculating the excess length of the extended guide rail, saw the rail and then weld it to the switch head; S8: after calculating the excess length of the extended guide rail, sawing the rail is performed, and then welding the rail with the upper rail of the turnout part and the lower rail of the turnout part is performed to release and lock the turnout; S9: After the release is completed, the turnout end is taken as the static end, and the welding of the turnout and its adjacent track is completed in sequence. After the construction is completed, the rails at both ends of the turnout are locked. At this time, the flash welding construction of the turnout rail joint is completed.

[0018] A construction method for flash welding of all rail joints of a turnout, characterized in that: in step S4 and step S6, the spacer irons and the stoppers are temporarily removed during the laying process.

[0019] A construction method for flash welding of all rail joints of a turnout, characterized in that step S7 is implemented by the following steps: S7.1: Measure the misalignment between the two rail tips and the adjacent control datums respectively, reserve the theoretical top forging burnout amount of the rail flash welding at the tail end of the extended curved upper rail and the extended straight lower rail, and saw off the excess rail at the head end of both rails. The length of the excess rail is the misalignment minus the theoretical top forging burnout amount of the rail flash welding, and ensure that the relative distance between the two rail tips is not more than 5 mm; S7.2: With the switch as the static end, complete the welding of the extended curved upper rail, the extended straight lower rail and the switch head in sequence, and resume the installation of fasteners, spacers and limiters.

[0020] A construction method for flash welding of all rail joints of a turnout, characterized in that step S8 is implemented by the following steps: S8.1: Loosen the fasteners of the upper rail and the lower rail of the turnout in sequence, saw off the excess rails at the tail of the extended upper rail and the extended lower rail, and reserve the theoretical top forging burnout amount of the rail flash welding as the loss of the rail welding. The excess rail length is the actual welding theoretical error value plus the surplus amount; S8.2: With the extended straight upper rail and the extended curved lower rail as the static ends, complete the welding of the extended straight upper rail and the straight upper rail of the switch section, and the extended curved lower rail and the curved lower rail of the switch section in sequence, and restore the fasteners; S8.3: Release the lock of the turnout within the locking rail temperature range.

[0021] A flash welding construction method for all rail joints of a turnout, characterized in that: AT rails are used at some welding points of the turnout, and when welding joints near the AT rails, the guide electrode of the flash welding is replaced by a guide electrode whose contact surface matches the waist surface of the AT rail.

[0022] During the specific implementation process, taking the P60-18# turnout as an example, firstly, 4 extended guide rails (extended straight upper rail, extended curved upper rail, extended straight lower rail and extended curved lower rail) are prepared to replace the original turnout rails, and the long rails of the same model and track type are used to saw the rails on the long rails according to the design length. Secondly, the welding upset error is controlled within ±2mm, and two flash welding guide electrodes that are coupled and matched with the AT rail structure dimensions are prepared. Since the turnout part can only be used as the static end during the flash welding process inside the turnout, the turnout end can only be used as the static end during the flash welding of the 6 joints outside the turnout, and the directions of different turnouts in the station are inconsistent, the mobile flash welding machine needs to be frequently turned to adjust the direction of the welding machine during construction. In order to avoid frequent turning, after the station has the conditions for turnout welding, each station arranges 2 welding machines with opposite directions for synchronous construction. After completing the construction of all the welding heads in the turnout of a station, it is transferred to the next station for construction.

[0023] The extended guide rail is an ordinary long rail that has been lengthened, while the point rail and switch are specially processed rail parts and are not easy to lengthen. In terms of the lengthening amount, the theoretical top forging burning amount of the rail flash welding is set to 35mm, the actual welding error value is set to 3mm, the joint rail gap value is set to 8mm, and the surplus amount is set to 10mm.

[0024] In the description of the present invention, it is necessary to understand that the indicated orientation or positional relationship is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0025] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A flash welding construction method for all rail joints of a turnout, comprising a turnout, wherein the turnout comprises a base rail, a point rail, an upper rail, a lower rail, a rudder rail and a rudder, wherein the base rail comprises a straight base rail and a curved base rail, the point rail comprises a straight point rail and a curved point rail, the upper rail comprises a straight upper rail and a curved upper rail, the lower rail comprises a straight lower rail and a curved lower rail, and the rudder rail comprises a rudder straight upper rail and a rudder curved lower rail; Features: It also includes an extended guide rail, which includes an extended straight upper guide rail, an extended curved upper guide rail, an extended straight lower guide rail and an extended curved lower guide rail of the same length, and the length of the extended guide rail = (theoretical top forging burnout amount of rail flash welding + actual welding theoretical error value + joint rail gap value + surplus amount) × 2; This method is implemented by the following steps: S1: Lay the rail components of the turnout, install the fasteners, and then adjust the internal structure dimensions of the turnout to meet the acceptance standards; S2: Mark the corresponding position of the tip of the pointed rail on the base rail as the control reference; S3: Remove the curved point rail and the curved upper strand guide rail, remove the straight upper strand guide rail and replace it with an extended straight upper strand guide rail, take the straight basic rail as the static end, complete the welding between it and the extended straight upper strand guide rail, and then install the fasteners of the extended straight upper strand guide rail; S4: weld the removed curved point rail and the extended curved upper rail outside the turnout, and then re-lay the curved point rail and the extended curved upper rail; S5: Remove the straight point rail and the straight lower rail, remove the curved lower rail and replace it with an extended curved lower rail, take the curved basic rail as the static end, complete the welding between it and the extended curved lower rail, and then install the fasteners of the extended curved lower rail; S6: weld the removed straight point rail and the extended straight down rail outside the turnout, and then re-lay the straight point rail and the extended straight down rail; S7: After calculating the excess length of the extended guide rail, saw the rail and then weld it to the switch head; S8: after calculating the excess length of the extended guide rail, sawing the rail is performed, and then welding the rail with the upper rail of the turnout part and the lower rail of the turnout part is performed to release and lock the turnout; S9: After the release is completed, the turnout end is taken as the static end, and the welding of the turnout and its adjacent track is completed in sequence. After the construction is completed, the rails at both ends of the turnout are locked. At this time, the flash welding construction of the turnout rail joint is completed.

2. A flash welding construction method for all rail joints of a turnout according to claim 1, characterized in that: In step S4 and step S6, the spacer irons and limiters are temporarily removed during the laying process.

3. A flash welding construction method for all rail joints of a turnout according to claim 1, characterized in that: Step S7 is implemented by the following steps: S7.1: Measure the misalignment between the two rail tips and the adjacent control datums respectively, reserve the theoretical top forging burnout amount of the rail flash welding at the tail end of the extended curved upper rail and the extended straight lower rail, and saw off the excess rail at the head end of both rails. The length of the excess rail is the misalignment minus the theoretical top forging burnout amount of the rail flash welding, and ensure that the relative distance between the two rail tips is not more than 5 mm; S7.2: With the switch as the static end, complete the welding of the extended curved upper rail, the extended straight lower rail and the switch head in sequence, and resume the installation of fasteners, spacers and limiters.

4. A flash welding construction method for all rail joints of a turnout according to claim 1, characterized in that: Step S8 is implemented by the following steps: S8.1: Loosen the fasteners of the upper rail and the lower rail of the turnout in sequence, saw off the excess rails at the tail of the extended upper rail and the extended lower rail, and reserve the theoretical top forging burnout amount of the rail flash welding as the loss of the rail welding. The excess rail length is the actual welding theoretical error value plus the surplus amount; S8.2: With the extended straight upper rail and the extended curved lower rail as the static ends, complete the welding of the extended straight upper rail and the straight upper rail of the switch section, and the extended curved lower rail and the curved lower rail of the switch section in sequence, and restore the fasteners; S8.3: Release the lock of the turnout within the locking rail temperature range.

5. A construction method for flash welding of all rail joints of a turnout according to claim 1, characterized in that: AT rails are used at some welding points of the turnout. When welding the joints near the AT rails, the guide electrode of the flash welding is replaced with a guide electrode whose contact surface matches the waist surface of the AT rail.

Citation Information

Cited By

  • Turnout steel rail flash welding method and welding construction method thereof

    CN120269301A

  • Construction method for transforming existing line turnout switch rail