Laser hybrid welding process for ship block construction

Through the laser composite welding process, combined with laser-MAG composite welding and double-wire submerged arc welding, the problems of low welding efficiency and large deformation of medium and thick plates in ship segment construction are solved, and efficient and stable welding quality and cost savings are achieved.

CN118989598AActive Publication Date: 2024-11-22CHINA MERCHANTS HEAVY IND JIANGSU +1

Patent Information

Application Number
CN202411237151.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The welding efficiency of existing ships in section construction medium and thick plates is low, the welding deformation and stress are high, the welding quality is not high, and the consumables cost is high.

Method used

The laser composite welding process is adopted, including laser-MAG composite welding and double-wire submerged arc welding. The front weld and longitudinal bone material are double-face symmetrical welding through laser arc composite welding equipment, combining hydraulic compression and reverse deformation pre-bending treatment. Achieve efficient welding.

Benefits of technology

The welding efficiency of ship segmented thick plate panels has been greatly improved, significantly reduced welding deformation and stress, improved welding quality, saved consumable costs, and achieved full penetration welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989598A_ABST
    Figure CN118989598A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of welding, and discloses a ship block building laser hybrid welding process which comprises the following steps: firstly, welding a front welding seam of a block jointed board seam through laser arc hybrid welding equipment to form a large block sheet; after welding of the front welding seam of the jointed board seam is completed, assembling and welding of the longitudinal aggregate are conducted through laser-electric arc hybrid welding equipment; after the longitudinal aggregate is completed, fillet welds of the transverse T-row structure are welded through a full-automatic robot flux-cored wire gas shielded welding process, and other small supporting web structural parts are welded through semi-automatic flux-cored wire gas shielded welding; and after the sections are turned over, a double-wire submerged-arc welding process is adopted for welding a reverse welding seam of the jointed board seam. The thick plate welding device is used for thick plate welding for ship block construction, the welding production efficiency can be greatly improved when the thick plate welding device is used for thick plate welding, welding deformation and welding stress can be remarkably reduced in the block manufacturing process, the welding quality is high, meanwhile, the welding consumable cost is greatly saved, and the thick plate welding for ship block construction has the great advantage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, in particular to a laser composite welding process for ship segment construction. Background Art

[0002] With the development of the global shipping industry, the demand for shipbuilding is increasing. In the process of ship block construction, the welding production volume is large, the welds are dense, and the welding man-hours account for a large proportion. In addition, for full penetration welds such as panel seams, the weld quality requirements are high, and generally there are requirements for post-weld flaw detection.

[0003] At present, for the welding of thick plates in the construction of ships in sections, the shipyards commonly use submerged arc welding or FCB welding for butt welding of panels, and CO2 gas shielded welding for longitudinals and T-row fillet welds. Among them, submerged arc welding for thick plate welding has stable welding quality, but it requires multi-layer and multi-pass welding, and the welding efficiency is relatively low; FCB panel welding has high efficiency, but it is easy to produce welding crack defects, affecting the welding quality, and due to the characteristics of single-sided welding, the deformation after welding is large, generally requiring pyrotechnic correction; CO2 gas shielded welding for longitudinals and T-row fillet welds has low welding efficiency.

[0004] In the document ZL202211297009, a painted laser composite welding method for thin plate paneling is disclosed, which provides two plates to be butt-welded, and coats high temperature shop primers on at least the upper and lower surfaces of the two plates to be welded, respectively. The color of the high temperature shop primer is different from the color of the plates to be welded; the weld is tracked and positioned by an optical camera tracking device, and the optical camera tracking device obtains the color difference between the gap between the two plates to be welded and the high temperature shop primer to determine the weld position, and the two plates to be welded are welded and connected by laser composite welding. This method has low production efficiency, and increases welding deformation and welding stress.

[0005] Therefore, a new technical solution is needed to solve the above technical problems. Summary of the invention

[0006] In order to solve the above problems, the thick plate welding used for ship block construction can greatly improve the welding production efficiency, significantly reduce welding deformation and welding stress during the block production process, have high welding quality, and greatly save welding consumables costs. The thick plate welding used for ship block construction has great advantages. The present invention discloses a ship block construction laser composite welding process, including the following steps: Step a: First, the segmented plate seams are welded by laser arc hybrid welding equipment to form large segmented plates; Step 1: Preparation of bevel of panel joint: Use I-type bevel to automatically mill the bevel of two large plates placed on the steel platform. The circular milling cutter is in the middle of the two large plates to process the two bevel edges at the same time. After the milling is completed, the two large plates are automatically assembled and matched. The two large plates are close together to ensure that the joint gap is no more than 1mm, and the hydraulic piano key device is used to press and fix them; Step 2: Preparation before seam welding: Check the laser protection lens to ensure it is smooth and pollution-free; check the welding protection gas, and verify the laser head position, MAG welding gun position, and filament spacing on the reference table; Step 3: Laser welding positioning of panel seams: pure laser welding is used for positioning welding; Step 4: Laser hybrid welding of the front weld of the panel seam: laser-MAG hybrid welding process is used to weld the front weld of the panel seam; Step b: After the front weld of the panel seam is welded, the longitudinal frame is assembled and welded using laser arc hybrid welding equipment; Step 1: Longitudinal frame assembly: Mechanical positioning, use hydraulic pressing tooling to press the frame, the frame and the base plate are close to each other, ensure that the joint gap is no more than 1mm, and use hydraulic lifting tooling to perform anti-deformation pre-bending treatment on the base plate; Step 2: Preparation before welding of longitudinal frame fillet weld: Check the laser protection lens to ensure it is smooth and pollution-free; check the welding shielding gas, and verify the laser head position, MAG welding gun position, and light wire spacing on the reference table; Step 3: Laser hybrid welding of longitudinal frame fillet weld: Laser-MAG hybrid welding process is used for double-sided symmetrical welding. The laser-MAG hybrid welding process involves double-sided welding guns and laser heads. Step c: After the longitudinal frame is completed, the fillet welds of the transverse T-row structure are welded by a fully automatic robot flux-cored gas-shielded welding process, and other small supporting web structural parts are welded by a semi-automatic flux-cored gas-shielded welding process; Step d: After turning over in sections, use double-wire submerged arc welding process to weld the reverse side weld of the joint.

[0007] Preferably, the laser beam and the front end of the welding wire used in step a are in a straight line with the plate seam, the laser head is perpendicular to the plate, the MAG welding gun is at a 45° angle to the plate, and is in an arc dragging posture, the length of the tack weld in step 3 is 300-500mm, and the number of tack welds for each panel seam is not less than 3; the laser power of the tack weld is 5~8KW, the defocus is -5~-8mm, and the welding speed is 3~4m / min.

[0008] Preferably, the laser head used in step b is at an angle of 25° to the base plate, the MAG welding gun is at an angle of 45° to the base plate, and is in an arc dragging posture. The laser beam is 1 to 2 mm above the intersection of the base plate and the vertical plate, and the front end of the welding wire is at the intersection of the base plate and the vertical plate. At this time, the extended length of the welding wire is 22 mm.

[0009] Preferably, step 2 in step b uses an Ar-CO2 mixed gas, the ratio of Ar to CO2 is 92:8, and the flow rate is 40~50L / min.

[0010] Preferably, the distance between the double-sided welding guns in step b and step 3 is 100-200 mm, and the welding parameters used are as follows: the laser power is 4-6 KW, the defocus is 0-2 mm, and the light wire distance is 0-2 mm.

[0011] Preferably, the MAG welding current is 250~280A, the welding voltage is 28~32V, the wire feeding speed is 10~12m / min, the welding speed is 2.5~3.5m / min, and the laser-MAG composite welding uses a solid welding wire with a diameter of 1.2~1.4mm, which is suitable for laser composite welding high-speed welding. The selected welding wire deposited metal composition is: C, 0.04~0.08%; Si, 0.6~1.2%; Mn, 1.3~1.6%; P, <0.020%; S, <0.015%; Ni, 0.2~0.8%.

[0012] Preferably, the double-wire submerged arc welding process in step d uses a submerged arc welding wire with a diameter of 4.0~5.0 mm, and the selected welding wire and flux have the following deposited metal components: C, 0.01~0.04%; Si, 0.2~0.4%; Mn, 1.2~2.0%; P, <0.020%; S, <0.015%; Cr, 0.01~0.05%; Mo, 0.01~0.03%; Ni, 0.3~1.0%.

[0013] By adopting the above technical solution, the welding material has stable mechanical properties under the condition of double-wire high heat input welding.

[0014] Preferably, the laser arc hybrid welding equipment includes a fiber laser and a pulse welding power supply, and the laser arc hybrid method is that the MAG welding gun is in front and the laser head is in the back, and the laser head and the MAG welding gun move straight forward without swinging the arc.

[0015] Preferably, the double-wire submerged arc welding equipment used in the double-wire submerged arc welding process in step d includes two welding power supplies, an AC power supply and a DC power supply. The two welding wires are arranged longitudinally, the front wire is tilted forward by 8 to 9 degrees, the rear wire is tilted backward by 15 degrees, the welding wire spacing is 20-30 mm, the two welding wires maintain the same straightness with the center of the plate seam, and a common molten pool is used during welding.

[0016] Preferably, the welding parameters used in step d are as follows: the front wire is DC, the welding current is 1000~1100A, and the welding voltage is 32~35V; the rear wire is AC, the welding current is 800~900A, the welding voltage is 38~40V, and the welding speed is 0.9~1.2m / min.

[0017] The benefits of the present invention are as follows: 1. It greatly improves the welding efficiency of ship segmented thick plate splicing. No beveling is done and a double-sided single-pass welding process is adopted. The maximum thickness can reach 30 mm. In addition, the welding process adopted has a fast welding speed. The maximum welding speed of the front laser-MAG composite welding process can reach 2.5 m / min, and the maximum welding speed of the back double-wire submerged arc welding process can reach 1.2 m / min. The production efficiency of thick plate splicing welding is greatly improved.

[0018] 2. The welding efficiency of longitudinal bone fillet welding is greatly improved. The laser-MAG composite welding process is used for double-sided symmetrical welding. The welding speed can reach up to 3.5m / min, which is 4 to 7 times that of ordinary gas shielded welding process, thus improving the production efficiency of longitudinal bone fillet welding.

[0019] 3. Greatly save welding materials. Full penetration welding can be achieved without beveling for panels with a thickness of 30 mm or less. The size of the beveling required for panels with a thickness of more than 30 mm is also greatly reduced compared with ordinary welding processes, which greatly saves the welding materials that need to be filled and saves the cost of welding consumables.

[0020] 4. The welding deformation is small during the segmented welding process, the welding quality is stable, and the cost of deformation correction is saved. The front weld of the panel is a laser-MAG composite welding process, with small welding heat input and small welding deformation; the back weld of the panel is a double-wire submerged arc welding process, which is carried out after the welding of the longitudinal bones, T-rows and other structural parts is completed, which has a greater constraint on the welding joints, so the welding deformation is also small; before the longitudinal frame fillet welding, the hydraulic jacking tooling is used to pre-bend the bottom plate for anti-deformation, so the deformation of the longitudinal bone fillet welding is also small.

[0021] 5. Optimize welding material matching. Laser-MAG composite welding selects solid welding wire with appropriate alloy composition, which is suitable for high-speed laser welding, ensuring the welding processability and mechanical properties of the welded joint under high-speed welding conditions; the submerged arc welding wire and flux used in double-wire submerged arc welding are alloy-strengthened to a certain extent, and 0.3~1.0% Ni element is added to ensure the low-temperature impact toughness of the welded joint under high heat input welding conditions, which can make the welded joint have good resistance to welding stress. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a flow chart of a welding process provided by an embodiment of the present invention; Figure 2 Schematic diagram of the positions of a MAG welding gun and a laser head relative to a plate seam of a laser composite welding tailored plate seam provided in an embodiment of the present invention; Figure 3 It is a schematic diagram of the positions of a MAG welding gun and a laser head relative to a base plate and a vertical plate for laser composite welding of longitudinal frames provided in an embodiment of the present invention.

[0023] in, Figure 2 and Figure 3 middle: Plate seam 100; laser beam 200; MAG welding wire 300; bottom plate 400; vertical plate 500; α1 Wire spacing; α2 Distance between laser beam and base plate; β1 Angle between MAG welding wire and plate seam; β2 Angle between laser beam and base plate; β3 Angle between MAG welding wire and base plate. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0025] like Figure 1 As shown, a laser composite welding process for ship block construction, with a plate thickness of 30 mm and a longitudinal bone thickness of 15 mm, comprises the following steps: Step a: First, the segmented plate seams are welded by laser arc hybrid welding equipment to form large segmented plates; Step 1: Preparation of bevel of panel joint: Use I-type bevel to automatically mill the bevel of two large plates placed on the steel platform. The circular milling cutter is in the middle of the two large plates to process the two bevel edges at the same time. After the milling is completed, the two large plates are automatically assembled and matched. The two large plates are close together to ensure that the joint gap is no more than 1mm, and the hydraulic piano key device is used to press and fix them; Step 2: Preparation before seam welding: Check the laser protection lens to ensure it is smooth and pollution-free; Check the welding shielding gas, verify the laser head position, MAG welding gun position, and light wire spacing on the reference table, check the surface condition of the steel plate, and remove water rust, paint, iron filings, and dust in the welding area and the range of 20mm wide on both sides; Check the surface condition of the welding wire, and replace the rusted welding wire with a new one; Check the extension length of the welding wire to ensure that the wire length is between 20mm. Too long or too short will affect the arc welding; Step 3: Laser welding positioning of panel seams: pure laser welding is used for positioning welding; Step 4: Laser hybrid welding of the front weld of the panel seam: laser-MAG hybrid welding process is used to weld the front weld of the panel seam; Step b: After the front weld of the panel seam is welded, the longitudinal frame is assembled and welded using laser arc hybrid welding equipment; Step 1: Longitudinal frame assembly: Mechanical positioning, use hydraulic pressing tooling to press the frame, the frame and the base plate are close to each other, ensure that the joint gap is no more than 1mm, the best is 0.5mm, and use hydraulic lifting tooling to pre-bend the base plate; Step 2: Preparation before welding of longitudinal frame fillet weld: Check the laser protection lens to ensure it is smooth and pollution-free; check the welding shielding gas, and verify the laser head position, MAG welding gun position, and light wire spacing on the reference table; Step 3: Laser hybrid welding of longitudinal frame fillet weld: Laser-MAG hybrid welding process is used for double-sided symmetrical welding. The laser-MAG hybrid welding process involves double-sided welding guns and laser heads. Step c: After the longitudinal frame is completed, the fillet welds of the transverse T-row structure are welded by a fully automatic robot flux-cored gas-shielded welding process, and other small supporting web structural parts are welded by a semi-automatic flux-cored gas-shielded welding process; Step d: After turning over in sections, use double-wire submerged arc welding process to weld the reverse side weld of the joint.

[0026] The front end of the laser beam and welding wire used in step a is in a straight line with the plate seam, the laser head is perpendicular to the plate, the MAG welding gun is at a 45° angle to the plate, and is in a drag arc posture. The length of the positioning weld in step 3 is 300mm, and the number of positioning welds for each joint seam is not less than 3; the laser power of the positioning weld is 8KW, the defocus is -8mm, and the welding speed is 3m / min; The laser head used in step b is at a 25° angle to the base plate, the MAG welding gun is at a 45° angle to the base plate, and is in an arc dragging posture. The laser beam is 2mm above the intersection of the base plate and the vertical plate, and the front end of the welding wire is at the intersection of the base plate and the vertical plate. At this time, the extended length of the welding wire is 22mm.

[0027] Preferably, step 2 in step b uses an Ar-CO2 mixed gas, the ratio of Ar to CO2 is 92:8, and the flow rate is 45 L / min.

[0028] In step b, the distance between the double-sided welding guns in step three is 200 mm, and the welding parameters used are as follows: the laser power is 6 KW, the defocus is -2 mm, and the light wire distance is 2 mm.

[0029] The MAG welding current is 280A, the welding voltage is 32V, the wire feeding speed is 12m / min, the welding speed is 3m / min, and the laser-MAG composite welding uses a solid welding wire with a diameter of 1.2, which is suitable for laser composite welding high-speed welding. The selected welding wire deposited metal composition is: C, 0.05%; Si, 0.8%; Mn, 1.5%; P, 0.015%; S, 0.012%; Ni, 0.3%.

[0030] In step d, the double-wire submerged arc welding process uses a submerged arc welding wire with a diameter of 5.0 mm. The selected welding wire and flux have the following deposited metal components: C, 0.02%; Si, 0.3%; Mn, 1.6%; P, 0.016%; S, 0.01%; Cr, 0.03%; Mo, 0.03%; Ni, 0.6%. This welding material has stable mechanical properties under the condition of double-wire high heat input welding.

[0031] The laser arc hybrid welding equipment includes a fiber laser and a pulse welding power supply. The laser arc hybrid method is that the MAG welding gun is in front and the laser head is in the back. The laser head and the MAG welding gun move straight without swinging the arc.

[0032] When laser hybrid welding is performed on the front weld of a panel seam, the positions of the MAG welding wire 300 and the laser beam 200 relative to the panel seam 100 are as follows: Figure 2 As shown, the front end of the laser beam 200 and the MAG welding wire 300 are in a straight line with the plate seam 100, the laser beam 200 is perpendicular to the plate, the angle β1 between the MAG welding wire 300 and the plate seam 100 is 45°, and it is in an arc dragging posture, and the wire spacing α1 is 2 mm.

[0033] When laser hybrid welding the longitudinal fillet weld, the positions of the MAG welding wire 300 and the laser beam 200 relative to the bottom plate 400 and the vertical plate 500 are as follows: Figure 3 As shown, the angle β2 between the laser beam 200 and the bottom plate 400 is 25°, the angle β3 between the MAG welding wire 300 and the bottom plate 400 is 45°, and the MAG welding wire 300 is in a dragging arc posture. The distance α2 above the intersection of the bottom plate 400 and the vertical plate 500 of the laser beam 200 is 2 mm, and the front end of the MAG welding wire 300 is at the intersection of the bottom plate 400 and the vertical plate 500. At this time, the wire extension length is 22 mm.

[0034] The double-wire submerged arc welding equipment used in the double-wire submerged arc welding process in step d includes two welding power supplies, an AC power supply and a DC power supply. The two welding wires are arranged longitudinally, the front wire is tilted forward by 9°, the rear wire is tilted backward by 15°, the welding wire spacing is 30 mm, the two welding wires maintain the same straightness with the center of the plate seam, and a common molten pool is used during welding.

[0035] The 30mm thick joint of the panel can be welded by welding one weld on the front and back sides, and full penetration can be achieved.

[0036] The 15-thick longitudinal frame fillet weld can be completed by welding one weld on each side. This fillet weld has a large penetration depth and a small weld foot, which is only 3mm.

[0037] By optimizing the laser composite welding process, full penetration welding can be achieved by using a double-sided single-pass welding process without beveling for panels with a thickness of 30 mm or less, and the welding speed is fast and the welding deformation is small. Compared with conventional welding processes, the laser composite welding process for ship segment construction provided by the present invention can greatly improve the welding production efficiency for thick plate welding, significantly reduce welding deformation and welding stress during segment production, and has high welding quality. At the same time, it greatly saves the cost of welding consumables, and has great advantages in being applied to thick plate welding for ship segment construction.

[0038] It should be understood by those skilled in the art that the embodiments of the present invention described above and shown in the accompanying drawings are only examples and do not limit the present invention, and the purpose of the present invention has been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. A laser composite welding process for ship segment construction, characterized in that: The following steps are involved: Step a: First, the segmented plate seams are welded by laser arc hybrid welding equipment to form large segmented plates; Step 1: Preparation of bevel of panel joint: Use I-type bevel to automatically mill the bevel of two large plates placed on the steel platform. The circular milling cutter is in the middle of the two large plates to process the two bevel edges at the same time. After the milling is completed, the two large plates are automatically assembled and matched. The two large plates are close together to ensure that the joint gap is no more than 1mm, and the hydraulic piano key device is used to press and fix them; Step 2: Preparation before seam welding: Check the laser protection lens to ensure it is smooth and pollution-free; check the welding protection gas, and verify the laser head position, MAG welding gun position, and filament spacing on the reference table; Step 3: Laser welding positioning of panel seams: pure laser welding is used for positioning welding; Step 4: Laser hybrid welding of the front weld of the panel seam: laser-MAG hybrid welding process is used to weld the front weld of the panel seam; Step b: After the front weld of the panel seam is welded, the longitudinal frame is assembled and welded using laser arc hybrid welding equipment; Step 1: Longitudinal frame assembly: Mechanical positioning, use hydraulic pressing tooling to press the frame, the frame and the base plate are close to each other, ensure that the joint gap is no more than 1mm, and use hydraulic lifting tooling to perform anti-deformation pre-bending treatment on the base plate; Step 2: Preparation before welding of longitudinal frame fillet weld: Check the laser protection lens to ensure it is smooth and pollution-free; check the welding shielding gas, and verify the laser head position, MAG welding gun position, and light wire spacing on the reference table; Step 3: Laser hybrid welding of longitudinal frame fillet weld: Laser-MAG hybrid welding process is used for double-sided symmetrical welding. The laser-MAG hybrid welding process involves double-sided welding guns and laser heads. Step c: After the longitudinal frame is completed, the fillet welds of the transverse T-row structure are welded by a fully automatic robot flux-cored gas-shielded welding process, and other small supporting web structural parts are welded by a semi-automatic flux-cored gas-shielded welding process; Step d: After turning over in sections, use double-wire submerged arc welding process to weld the reverse side weld of the joint.

2. A laser hybrid welding process for ship segment construction according to claim 1, characterized in that: The laser beam and the front end of the welding wire used in step a are in a straight line with the plate seam, the laser head is perpendicular to the plate, the MAG welding gun is at a 45° angle to the plate, and is in a drag arc posture. The length of the positioning weld in step 3 is 300-500mm, and the number of positioning welds for each joint seam is not less than 3; the laser power of the positioning welding is 5-8KW, the defocus is -5-8mm, and the welding speed is 3-4m / min.

3. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The laser head used in the step b is at an angle of 25° to the base plate, the MAG welding gun is at an angle of 45° to the base plate, and is in an arc dragging posture. The laser beam is 1 to 2 mm above the intersection of the base plate and the vertical plate, and the front end of the welding wire is at the intersection of the base plate and the vertical plate. At this time, the extended length of the welding wire is 22 mm.

4. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The second step in step b uses Ar-CO2 mixed gas, the ratio of Ar to CO2 is 92:8, and the flow rate is 40-50 L / min.

5. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The distance between the double-sided welding guns in step 3 of step b is 100-200 mm, and the welding parameters used are as follows: the laser power is 4-6 KW, the defocus is 0--2 mm, and the light wire distance is 0-2 mm.

6. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The MAG welding current is 250-280A, the welding voltage is 28-32V, the wire feeding speed is 10-12m / min, the welding speed is 2.5-3.5m / min, the laser-MAG composite welding adopts a solid welding wire with a diameter of 1.2-1.4mm, which is suitable for laser composite welding high-speed welding. The selected welding wire deposited metal composition is: C, 0.04-0.08%; Si, 0.6-1.2%; Mn, 1.3-1.6%; P, <0.020%; S, <0.015%; Ni, 0.2-0.8%.

7. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The double-wire submerged arc welding process in step d adopts a submerged arc welding wire with a diameter of 4.0-5.0 mm, and the selected welding wire and flux have the following deposited metal components: C, 0.01-0.04%; Si, 0.2-0.4%; Mn, 1.2-2.0%; P, <0.020%; S, <0.015%; Cr, 0.01-0.05%; Mo, 0.01-0.03%; Ni, 0.3-1.0%.

8. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The laser arc hybrid welding equipment comprises a fiber laser and a pulse welding power supply. The laser arc hybrid welding mode is that the MAG welding gun is in front and the laser head is in the back. The laser head and the MAG welding gun move straightly without arc swing.

9. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The double-wire submerged arc welding equipment used in the double-wire submerged arc welding process in step d includes two welding power sources, an AC power source and a DC power source. The two welding wires are arranged longitudinally, the front wire is tilted forward by 8 to 9 degrees, the rear wire is tilted backward by 15 degrees, the welding wire spacing is 20 to 30 mm, the two welding wires maintain the same straightness with the center of the plate seam, and a common molten pool is used during welding.

10. The laser hybrid welding process for ship segment construction according to claim 1 is characterized by: The welding parameters used in step d are as follows: the front wire is DC, the welding current is 1000-1100A, and the welding voltage is 32-35V; the rear wire is AC, the welding current is 800-900A, the welding voltage is 38-40V, and the welding speed is 0.9-1.2m / min.

Citation Information

Patent Citations

  • Segmental assembling and welding method of stem

    CN101987401A

  • Segmental construction method for thick plates of ships

    CN108098178A

  • Folded welding process of ultra-large ore carrying vessel main deck

    CN109746552A

  • All-position consumable electrode arc-laser double-sided hybrid welding process and equipment

    CN111872563A

  • Method for single-side welding of thick plate for ship

    CN112453707A

Cited By

  • Method for controlling segmented deformation of thin plate of PCTC large roll-on-roll-off ship

    CN121180410A