Hot-bending microcrystalline glass and preparation method thereof

By controlling the ratio of glass frit A and material B, microcrystalline glass with suitable temperature difference of softening point and crystallization peak is prepared, which solves the problem of crystal phase transition during thermal bending, improves light transmittance and mechanical properties, and is suitable for 2.5D-3D cover glass preparation.

CN118993547AActive Publication Date: 2024-11-22JIANGSU XIUQIANG GLASSWORK CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310550482.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

During the preparation of 2.5D-3D cover glass, conventional microcrystalline glass is prone to secondary crystallization during hot bending, affecting its light transmittance and mechanical strength, resulting in unstable performance.

Method used

Different proportions of glass frit A and glass frit B, including SiO2, Al2O3, Li2O, ZrO2, P2O5, B2O3 and other components, were used to prepare the basic glass by two-step method, and the temperature difference between the softening point and crystallization peak temperature was controlled at 70℃. Within the range of -110℃, expand the thermal bending temperature range to avoid crystal phase transformation.

Benefits of technology

It improves the light transmittance and mechanical properties of hot-bending microcrystalline glass, avoids unstable performance, is suitable for the preparation of 2.5D-3D cover glass, and improves the flexibility of the production process and the utilization rate of glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993547A_ABST
    Figure CN118993547A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: firstly, respectively preparing a glass material A and a glass material B from materials in different proportions, then controlling the proportion of the glass material A to the glass material B within a certain range to prepare base glass, and crystallizing, grinding and polishing the base glass to obtain the hot-bending glass ceramic. The base glass is prepared by adopting a two-step method, and the ratio of the frit A to the frit B is strictly controlled, so that the temperature difference between the softening point and the devitrification peak temperature of the microcrystalline glass can be controlled within the range of 70-110 DEG C, the adjustable temperature range in the hot bending process is expanded, the light transmittance of the hot-bending microcrystalline glass is improved, and the thermal conductivity of the microcrystalline glass is improved. The method avoids crystal phase transformation or disappearance of the microcrystalline glass in the hot bending process, avoids unstable performance after hot bending treatment, and is suitable for preparation of 2.5 D-3D cover plate glass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of microcrystalline glass, and in particular to a heat-bendable microcrystalline glass and a preparation method thereof. Background Art

[0002] With the advent of the flexible AMOLED and 5G era, 3D curved surface and glass materials have become standard configurations for mobile phones. Currently, plastic, ceramic, glass and metal can be used to make mobile phone shells. Plastic shells are limited to low-end mobile phones and have been basically eliminated; ceramic back covers have low production and higher prices, and large-scale production and yield are its biggest bottlenecks. Traditional metal shells naturally have the defect of shielding mobile phone signals. With the advent of the 5G era, wireless frequency bands will become more and more complex, and the requirements for signals will become higher and higher. Mobile phone antennas are generally installed on the back of mobile phones. Therefore, for the protection of signals, mobile phones are required to avoid using metal back shells as much as possible, and glass has become the best choice. The development of cover glass has gone through a process from 2D to 2.5D and then to 3D. Different from the traditional glass cover processing technology, 2.5D-3D glass cover has added a hot bending process. The appearance material of the hot-bent glass is more superior, and it has more advantages in heat dissipation, glossiness and wear resistance. At the same time, the curved design and the curvature of the palm are more in line with ergonomic requirements.

[0003] Glass-ceramics, also known as glass ceramics, is a composite material containing a crystalline phase and a glass phase obtained by nucleating and crystallizing glass. The unique structure of glass-ceramics makes it different from glass and ceramics, and its properties are determined by the composition and quantity of the crystalline phase and the glass phase. According to its light transmittance, glass-ceramics can also be divided into transparent glass-ceramics and opaque glass-ceramics. As a type of glass-ceramics, transparent glass-ceramics has excellent properties, namely transparency and low expansion, so when the temperature changes, the volume changes very little. It is a new functional material with excellent thermal, mechanical, optical and chemical properties, and has been widely used in various fields.

[0004] In the prior art, the patent with publication number CN115893851A discloses a glass-ceramic and a preparation method thereof. In terms of mass fraction, the components of the glass-ceramic include SiO2 37% to 46%, Al2O3 27% to 35%, Na2O 12 to 20%, K2O 0 to 5%, TiO2 1 to 3%, ZrO2 4% to 8% and P2O 54% to 10%. The glass-ceramic prepared by the mass percentage of the components in this scheme has high transmittance and mechanical properties, and can meet the applicable requirements of cover glass. However, in the process of preparing 2.5D-3D cover glass, hot bending is an important step, which is completed using the softening point temperature of the glass. For glass-ceramics of conventional components, the softening point and the crystallization temperature are slightly different. Therefore, when the glass-ceramics are hot bent, secondary crystallization will inevitably occur, affecting the transmittance and mechanical strength of the glass-ceramics, reducing the stability of the glass-ceramics, and being unfavorable for subsequent applications.

[0005] In view of this, it is necessary to design a heat-bendable microcrystalline glass and a preparation method thereof to solve the above problems. Summary of the invention

[0006] The object of the present invention is to provide a heat-bendable microcrystalline glass and a preparation method thereof which has high light transmittance and can avoid crystal phase transition or disappearance during the heat bending process, and avoid unstable performance after the heat bending process, and is suitable for the preparation of 2.5D-3D cover glass.

[0007] To achieve the above-mentioned purpose, the present invention provides a heat-bendable microcrystalline glass, wherein the base glass comprises a certain proportion of glass material A and glass material B, wherein the glass material A comprises the following components: 65-75wt% SiO2, 4-8wt% Al2O3, 10-17wt% Li2O, 4-7wt% ZrO2, 3-5wt% P2O5, and 0-0.5wt% B2O3, and the glass material B comprises the following components: 40-55wt% SiO2, 14-20wt% Al2O3, and 0-2wt% L i2 O, 4~7wt% ZrO2, 0~3wt% P2O5, 2~6wt% K2O, 12~20wt% Na2O, 4~8wt% CaO, 0~0.5wt% B2O3, 0.2~2wt% BaO.

[0008] As a further improvement of the present invention, the mass ratio of the glass frit A to the glass frit B is (30-70): (70-30).

[0009] The present invention also provides a method for preparing heat-bendable microcrystalline glass according to any one of the above technical solutions, comprising the following steps:

[0010] S1. Weigh raw materials according to the components of glass material A, mix them well and add them into a crucible at 1500-1650° C., keep them warm for 4-8 hours to obtain glass liquid A, and obtain glass material A through infiltration, drying and sieving;

[0011] S2, weighing raw materials according to the components of glass frit B, mixing them well and adding them into a crucible at 1550-1680° C., keeping the temperature for 6-10 hours to obtain glass liquid B, and then obtaining glass frit B through infiltration, drying and sieving;

[0012] S3, weighing the glass material A prepared in step S1 and the glass material B prepared in step S2 in a mass ratio of (30-70): (70-30), mixing and sieving to obtain a mixture C, adding the mixture C into a crucible, keeping the mixture at a predetermined temperature for a certain period of time, stirring and annealing to obtain a basic glass;

[0013] S4. The base glass prepared in step S3 is crystallized, ground and polished to obtain heat-bendable microcrystalline glass.

[0014] As a further improvement of the present invention, in step S3, the predetermined temperature is 1500-1600°C, and the insulation time is 2-4h.

[0015] As a further improvement of the present invention, in step S3, the stirring operation is stirring at a speed of 4 to 12 rpm for 4 to 6 hours; the annealing operation is: pouring the stirred glass liquid into a mold at 400 to 420°C, and after the color of the glass darkens, placing the glass in an annealing furnace at 510 to 540°C, keeping it warm for 3 to 5 hours, and then cooling it to room temperature at a uniform speed over 12 to 24 hours.

[0016] As a further improvement of the present invention, in step S4, the crystallization operation is: placing the base glass into a crystallization furnace, uniformly heating the temperature to 520-540°C, keeping it warm for 1-2 hours, then uniformly heating the temperature to 640-680°C, keeping it warm for 4-24 hours, and then uniformly cooling the temperature to room temperature after 12-24 hours.

[0017] As a further improvement of the present invention, the particle size of the glass frit A and the glass frit B is greater than 1 mm.

[0018] As a further improvement of the present invention, in step S3, the sieve aperture used in the screening operation is 1 cm.

[0019] As a further improvement of the present invention, the heat-bendable microcrystalline glass prepared in step S4 is placed in a 2.5-3D mold, and a heat-bent microcrystalline glass product is obtained by heat-bending treatment.

[0020] As a further improvement of the present invention, the hot bending treatment operation is: placing the 2.5-3D mold containing the hot-bendable microcrystalline glass into a heating furnace with nitrogen as the protective gas, heating it uniformly to 580-620°C over 1-3 hours, and then using the upper mold to press and shape it for 5-10 seconds; then keeping it warm at 520-540°C for 10-30 minutes, and then cooling it uniformly to room temperature over 4-6 hours.

[0021] The beneficial effects of the present invention are:

[0022] 1. The present invention prepares a crystallizable glass material A and a non-crystallizable glass material B respectively by using materials in different proportions, and then controls the ratio of glass material A to glass material B within a certain range to prepare a basic glass, and performs crystallization, grinding and polishing treatments on the basic glass to obtain a heat-bendable microcrystalline glass. By adopting a two-step method to prepare the basic glass and strictly controlling the ratio of glass material A to glass material B, the temperature difference between the softening point of the microcrystalline glass and the crystallization peak temperature can be controlled within the range of 70°C-110°C, expanding the adjustable temperature range during the heat bending process, and improving the light transmittance of the heat-bent microcrystalline glass. Compared with conventional microcrystalline glass, the microcrystalline glass of the present invention can avoid the occurrence of crystal phase transition or disappearance during the heat bending process, and avoid the occurrence of unstable performance after the heat bending process, and is suitable for the preparation of 2.5D-3D cover glass.

[0023] 2. The two-step preparation design of the basic glass of the present invention can adjust the ratio of glass material A and glass material B to obtain microcrystalline glass that meets different hot bending requirements, quickly respond to 2.5D-3D preparation needs, and can flexibly adjust the opening and closing of the production line according to production tasks. The production process has high control accuracy and the glass utilization rate can reach more than 95%.

[0024] 3. The heat-bendable microcrystalline glass prepared by the preparation method of the present invention has a stable crystal phase, high dimensional accuracy, a smooth surface, and high glass transmittance. It can be widely used in aerospace technology, integrated circuit boards, solid lasers, infrared generators, infrared detection devices, high-temperature resistant cookers, high-temperature observation windows, and communication mobile terminal electronic equipment fields, and there is no need to increase the yield of heat-bendable glass by adding an external protective layer. At the same time, the preparation process of the present invention is simple, low-cost, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the differential thermal analysis result of the heat-bent glass-ceramics prepared in Example 1.

[0026] Figure 2 This is the expansion analysis result of the heat-bent glass-ceramics prepared in Example 1.

[0027] Figure 3This is the XRD test result of the heat-bent glass-ceramics prepared in Example 1.

[0028] Figure 4 This is the SEM test result of the heat-bent glass-ceramics prepared in Example 1.

[0029] Figure 5 This is the transmittance test result of the heat-bent microcrystalline glass prepared in Example 1. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0032] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0033] The present invention provides a heat-bendable microcrystalline glass, wherein the base glass comprises glass material A and glass material B in a mass ratio of (30-70): (70-30), wherein the glass material A comprises the following components: 65-75wt% SiO2, 4-8wt% Al2O3, 10-17wt% Li2O, 4-7wt% ZrO2, 3-5wt% P2O5, and 0-0.5wt% B2O3, and the glass material B comprises the following components: 40-55wt% SiO2, 14-20wt% Al2O3, 0-2wt% Li2O, 4-7wt% ZrO2, 0-3wt% P2O5, 2-6wt% K2O, 12-20wt% Na2O, 4-8wt% CaO, 0-0.5wt% B2O3, and 0.2-2wt% BaO.

[0034] The present invention also provides a method for preparing heat-bendable microcrystalline glass, comprising the following steps:

[0035] S1. Weigh the raw materials according to the components of glass material A, mix them well and add them into a quartz crucible at 1500-1650° C., keep them warm for 4-8 hours to obtain glass liquid A, then pour the glass liquid A into distilled water at room temperature, remove it, dry it, and sieve it to obtain glass material A with a particle size greater than 1 mm;

[0036] S2, weighing raw materials according to the components of glass material B, mixing them well, adding them into a quartz crucible at 1550-1680° C., and keeping them warm for 6-10 hours to obtain glass liquid B, then pouring the glass liquid B into distilled water at room temperature, taking it out, drying it, and sieving it to obtain glass material B with a particle size greater than 1 mm;

[0037] S3, weighing the glass material A prepared in step S1 and the glass material B prepared in step S2 in a mass ratio of (30-70): (70-30), mixing them, sieving them three times through a sieve with a pore size of 1 cm to obtain a mixture C, adding the mixture C into a platinum crucible at 1500-1600° C., keeping the mixture for 2-4 hours, stirring and annealing to obtain a basic glass;

[0038] S4. The base glass prepared in step S3 is crystallized, ground and polished to obtain heat-bendable microcrystalline glass.

[0039] Specifically, in step S3, the stirring operation is to stir at a speed of 4 to 12 rpm for 4 to 6 hours; the annealing operation is to pour the stirred glass liquid into a stainless steel mold at 400 to 420° C., and after the color of the glass darkens, place the glass in an annealing furnace at 510 to 540° C., keep it warm for 3 to 5 hours, and then cool it down to room temperature at a uniform speed after 12 to 24 hours.

[0040] Specifically, in step S4, the crystallization operation is as follows: the base glass is placed in a crystallization furnace, the temperature is uniformly increased from room temperature to 520-540°C over 4 hours, the temperature is kept at a constant rate for 1-2 hours, the temperature is uniformly increased to 640-680°C over 2 hours, the temperature is kept at a constant rate for 4-24 hours, and the temperature is uniformly decreased to room temperature over 12-24 hours.

[0041] Specifically, the grinding and polishing operations are: using diamond wire to cut the crystallized glass into glass sheets with a thickness of 0.2 to 10 mm, and then making flat crystallized glass sheets through rough grinding, fine grinding, polishing and other processes to obtain heat-bendable microcrystalline glass.

[0042] Specifically, the heat-bendable microcrystalline glass prepared in step S4 is placed in a 2.5-3D mold, and then placed in a heating furnace with nitrogen as the protective gas. After 1 to 3 hours, the temperature is uniformly increased to 580 to 620°C, and then the upper mold is used to press and shape for 5 to 10 seconds; at a temperature of 520-540°C, it is kept warm for 10 to 30 minutes, and then uniformly cooled to room temperature after 4 to 6 hours to obtain a heat-bent microcrystalline glass product.

[0043] The preparation method of the heat-bendable microcrystalline glass provided by the present invention is described below with reference to specific embodiments.

[0044] Example 1

[0045] This embodiment provides a method for preparing heat-bendable microcrystalline glass, comprising the following steps:

[0046] S1. Weigh 72wt% SiO2, 6wt% Al2O3, 13wt% Li2O, 4.5wt% ZrO2, 4wt% P2O5 and 0.5wt% B2O3 respectively, mix well and add into a quartz crucible at 1600°C, keep warm for 6 hours to obtain glass liquid A; then pour the glass liquid A into distilled water at room temperature, remove it, dry it and sieve it to obtain glass material A with a particle size greater than 1mm;

[0047] S2, respectively weigh 48wt% SiO2, 16wt% Al2O3, 1wt% Li2O, 5.5wt% ZrO2, 2wt% P2O5, 4wt% K2O, 16wt% Na2O, 6wt% CaO, 0.5wt% B2O3, 1wt% BaO, mix well and add into a quartz crucible at 1550°C, keep warm for 6 hours, and obtain glass liquid B; then pour the glass liquid B into distilled water at room temperature, take it out, dry it, and sieve it to obtain glass material B with a particle size greater than 1mm;

[0048] S3, weighing the glass material A prepared in step S1 and the glass material B prepared in step S2 in a mass ratio of 30:70, mixing, and sieving three times with a sieve with a pore size of 1 cm to obtain a mixture C; adding the mixture C to a platinum crucible at 1550° C., keeping it warm for 3 hours, and stirring it with a platinum stirring paddle at a speed of 4 to 12 rpm for 5 hours; pouring the stirred glass liquid into a stainless steel mold at 410° C., and after the color of the glass darkens, placing the glass in an annealing furnace at 530° C., keeping it warm for 4 hours, and then cooling it to room temperature at a uniform speed over 20 hours to obtain a basic glass;

[0049] S4. Put the basic glass prepared in step S3 into a crystallization furnace, uniformly heat it from room temperature to 530°C over 4 hours, keep it warm for 2 hours, then uniformly heat it to 640°C over 2 hours, keep it warm for 4 hours, and then uniformly cool it to room temperature over 20 hours to obtain crystallized glass; then use diamond wire to cut the crystallized glass into glass sheets with a thickness of 5 mm, and make them flat through rough grinding, fine grinding and polishing processes to obtain heat-bendable microcrystalline glass.

[0050] The prepared heat-bendable microcrystalline glass is placed in a 3D graphite mold, and then placed in a heating furnace with nitrogen as the protective gas. The temperature is uniformly raised to 620°C after 3 hours, and then the upper mold is used to press and shape for 10 seconds; finally, the 3D graphite mold is moved into a furnace at 530°C, kept warm for 30 minutes, and then uniformly cooled to room temperature after 6 hours to obtain a heat-bent microcrystalline glass product.

[0051] Embodiments 2 to 6

[0052] Examples 2 to 6 respectively provide a method for preparing a heat-bendable microcrystalline glass. Compared with Example 1, the ratios of glass material A and glass material B in Examples 2-6 are adjusted to 35:65, 40:60, 45:55, 50:50, and 70:30, respectively. At the same time, according to the melting temperature requirements of mixed materials in different proportions, the temperature of the platinum crucible in step S3 of Examples 2-6 is adjusted from 1550°C to 1560°C, 1570°C, 1580°C, 1590°C, and 1600°C, respectively. The remaining steps are consistent with Example 1 and are not repeated here.

[0053] Comparative Examples 1 to 3

[0054] Comparative Examples 1-3 respectively provide a method for preparing a heat-bendable microcrystalline glass. Compared with Example 1, Comparative Example 1 adjusts the two-step method for preparing the basic glass in Example 1 to a one-step method, that is, directly using the same raw materials as those in the example to prepare the microcrystalline glass. The specific operation is: weighing the raw materials of glass material A and glass material B respectively according to a proportion, mixing them in a mass ratio of 30:70 to obtain a mixture C, and the subsequent steps are consistent with Example 1;

[0055] In Comparative Examples 2-3, the ratios of glass material A and glass material B are adjusted to 20:80 and 80:20, respectively. The remaining steps are the same as those in Example 1 and will not be described in detail herein.

[0056] The heat-bendable microcrystalline glasses prepared in Examples 2-6 and Comparative Examples 1-3 were respectively used to prepare heat-bend microcrystalline glass products using the same method as in Example 1.

[0057] The relevant properties of the heat-bent glass-ceramics of Examples 1-6 and Comparative Examples 1-3 were tested, and the results are shown in Table 1; wherein the differential thermal analysis curve, expansion curve, X-ray diffractometer test results, scanning electron microscope test results and transmittance test results of the heat-bent glass-ceramics of Example 1 are shown in Table 1. Figure 1-Figure 5 shown.

[0058] Table 1 Test results of relevant properties of heat-bent glass-ceramics of Examples 1-6 and Comparative Examples 1-3

[0059]

[0060] The density of the heat-bent glass-ceramics of Example 1 obtained by the Archimedean method is 3.12 g / cm 3 .Depend on Figure 1 It can be seen that the crystallization peak temperature of the heat-bent glass-ceramics of Example 1 obtained by differential heating is 640°C; the softening point temperature obtained by thermal expansion is 560°C, and the linear expansion coefficient α is 7.82×10 -6 / ℃(50~450℃)( Figure 2); The crystallinity of the heat-bent glass-ceramics was 86.5% and the grain size was 2.1nm ( Figure 3 ); The crystals in the heat-bent glass-ceramics were observed by a JMS-5610LV scanning electron microscope to be spherical or quasi-spherical with a size of 1-10 nm and evenly distributed ( Figure 4 ).like Figure 5 As shown, the transmittance of the heat-bent glass-ceramics prepared in Example 1 in the visible light range tested by GD751 spectrophotometer is greater than 90.8% (thickness 0.68mm, after 550nm). It can be seen that the adjustable temperature range between the softening point temperature and the crystallization peak temperature of the heat-bent glass-ceramics prepared in Example 1 is 80°C, and the heat-bendable glass-ceramics prepared by the preparation method of the present invention is suitable for heat bending treatment, and the heat-bent glass-ceramics obtained after heat bending treatment has stable crystal phase, high dimensional accuracy, smooth surface, and high crystallinity and transmittance.

[0061] It can be seen from Table 1 that when the ratio of glass material A and glass material B increases from 30:70 to 70:30, the temperature difference between the softening point temperature and the crystallization peak temperature of the heat-bent microcrystalline glass prepared in Examples 1-6 increases from 80°C to 110°C, and the transmittance is greater than 90%, the crystallinity is greater than or equal to 76%, and the crystals in the heat-bent microcrystalline glass observed by a JMS-5610LV scanning electron microscope are uniformly distributed, and are 1-10nm spherical or quasi-spherical, indicating that the heat-bendable microcrystalline glass prepared by the preparation method of the present invention is suitable for heat bending treatment and still has good performance after heat bending treatment.

[0062] Compared with Example 1, the temperature difference between the softening point temperature and the crystallization peak temperature of the heat-bent microcrystalline glass prepared in Comparative Example 1 is reduced to 23°C. At the same time, the grain size is increased, the linear expansion coefficient is reduced, and the light transmittance is significantly reduced to only 37%, indicating that the heat-bendable microcrystalline glass prepared according to Comparative Example 1 will have a significant decrease in stability after heat bending treatment.

[0063] In addition, when the proportion of glass material A is too low, the crystals of the heat-bendable microcrystalline glass will increase, resulting in a low polishing rate and poor transmittance (Comparative Example 2); when the proportion of glass material A is high, it will affect the degree of crystallization of the heat-bendable microcrystalline glass, resulting in a low degree of crystallization, and thus unable to meet the performance requirements of 2.5-3D cover glass (Comparative Example 3).

[0064] In summary, the present invention discloses a heat-bendable microcrystalline glass and a preparation method thereof. By adopting a two-step method to prepare the basic glass and strictly controlling the ratio of glass material A and glass material B, the temperature difference between the softening point of the microcrystalline glass and the crystallization peak temperature can be controlled within the range of 70°C-110°C, expanding the adjustable temperature range during the heat bending process, and improving the light transmittance of the heat-bent microcrystalline glass. At the same time, the crystal phase transformation or disappearance during the heat bending process is avoided, and the performance instability after the heat bending process is avoided. It is suitable for the preparation of 2.5D-3D cover glass. The heat-bendable microcrystalline glass prepared by the preparation method of the present invention has a stable crystal phase, high dimensional accuracy, a smooth surface, and high glass transmittance. It can be widely used in aerospace technology, integrated circuit boards, solid lasers, infrared generators, infrared detection devices, high temperature resistant cookers, high temperature observation windows, and communication mobile terminal electronic equipment fields; at the same time, the preparation process of the present invention is simple, low cost, and there is no need to increase the yield of heat-bent glass by adding an external protective layer, which is suitable for industrial production.

[0065] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A heat-bendable glass-ceramic, characterized in that: The base glass comprises a certain proportion of glass frit A and glass frit B, wherein the glass frit A comprises the following components: 65-75wt% SiO2, 4-8wt% Al2O3, 10-17wt% Li2O, 4-7wt% ZrO2, 3-5wt% P2O5, and 0-0.5wt% B2O3, and the glass frit B comprises the following components: 40-55wt% SiO2, 14-20wt% Al2O3, and 0-2wt% Li2O. i2 O, 4~7wt% ZrO2, 0~3wt% P2O5, 2~6wt% K2O, 12~20wt% Na2O, 4~8wt% CaO, 0~0.5wt% B2O3, 0.2~2wt% BaO.

2. The heat-bendable glass-ceramic according to claim 1, characterized in that: The mass ratio of the glass frit A to the glass frit B is (30-70):(70-30).

3. A method for preparing heat-bendable glass-ceramics according to any one of claims 1 to 2, characterized in that: The steps include: S1. Weigh raw materials according to the components of glass material A, mix them well and add them into a crucible at 1500-1650° C., keep them warm for 4-8 hours to obtain glass liquid A, and obtain glass material A through infiltration, drying and sieving; S2, weighing raw materials according to the components of glass frit B, mixing them well and adding them into a crucible at 1550-1680° C., keeping the temperature for 6-10 hours to obtain glass liquid B, and then obtaining glass frit B through infiltration, drying and sieving; S3, weighing the glass material A prepared in step S1 and the glass material B prepared in step S2 in a mass ratio of (30-70): (70-30), mixing and sieving to obtain a mixture C, adding the mixture C into a crucible, keeping the mixture at a predetermined temperature for a certain period of time, stirring and annealing to obtain a basic glass; S4. The base glass prepared in step S3 is crystallized, ground and polished to obtain heat-bendable microcrystalline glass.

4. The method for preparing heat-bendable glass-ceramics according to claim 3, characterized in that: In step S3, the predetermined temperature is 1500-1600°C, and the insulation time is 2-4h.

5. The method for preparing heat-bendable glass-ceramics according to claim 4, characterized in that: In step S3, the stirring operation is to stir at a speed of 4 to 12 rpm for 4 to 6 hours; the annealing operation is to pour the stirred glass liquid into a mold at 400 to 420° C., and after the color of the glass darkens, place the glass in an annealing furnace at 510 to 540° C., keep it warm for 3 to 5 hours, and then cool it down to room temperature at a uniform speed over 12 to 24 hours.

6. The method for preparing heat-bendable glass-ceramics according to claim 3, characterized in that: In step S4, the crystallization operation is as follows: placing the base glass into a crystallization furnace, uniformly heating the temperature to 520-540°C, keeping the temperature for 1-2 hours, then uniformly heating the temperature to 640-680°C, keeping the temperature for 4-24 hours, and then uniformly cooling the temperature to room temperature after 12-24 hours.

7. The method for preparing heat-bendable glass-ceramics according to claim 3, characterized in that: The particle sizes of the glass frit A and the glass frit B are greater than 1 mm.

8. The method for preparing heat-bendable glass-ceramics according to claim 3, characterized in that: In step S3, the sieve used in the screening operation has an aperture of 1 cm.

9. The method for preparing heat-bendable glass-ceramics according to claim 3, characterized in that: The heat-bendable microcrystalline glass prepared in step S4 is placed in a 2.5-3D mold, and a heat-bent microcrystalline glass product is obtained by heat-bending treatment.

10. The method for preparing heat-bendable glass-ceramics according to claim 9, characterized in that: The heat bending treatment operation is as follows: placing the 2.5-3D mold containing the heat-bendable microcrystalline glass into a heating furnace with nitrogen as the protective gas, heating it uniformly to 580-620°C over 1-3 hours, and then using the upper mold to press and shape it for 5-10 seconds; then keeping it at 520-540°C for 10-30 minutes, and then cooling it uniformly to room temperature over 4-6 hours.

Citation Information

Patent Citations

  • Glass composition, glass slurry containing glass composition, vacuum glass containing glass composition, resistor containing glass composition and preparation method

    CN109264988A

  • Low-loss low-temperature co-fired ceramic green tape and preparation method thereof

    CN113045204A

  • High-frequency low-loss LTCC substrate material capable of being electroplated or chemically plated, and preparation method thereof

    CN113213949A

  • Three-dimensional microcrystalline glass and preparation method thereof

    CN113248152A

  • 3D microcrystalline glass as well as preparation method and application thereof

    CN114790085A