Host-guest phosphorescent compound as well as preparation and application thereof
By synthesizing aromatic compounds with bromine chains and trimethylamine to form ammonium salts and doping them into PVA, adjustable luminescence phosphorescent polymers are prepared, which solves the problem of poor water solubility of organophosphorescence materials and achieves high efficiency in aqueous solution Phosphorescence material preparation and multi-layer information encryption effect.
Patent Information
- Application Number
- CN202411180198.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
AI Technical Summary
The application of existing organophosphorescence materials in aqueous solutions is limited by their fat solubility, resulting in poor water solubility, which limits their application in the fields of information storage, encryption and biological imaging.
By synthesizing aromatic compounds with bromine chains and reacting with trimethylamine to form ammonium salts, doping them into polymer PVA, phosphorescent polymers that can adjust the luminescent color and life are prepared, and compounded with cucurbitum or cyclodextrin to form a pyrogenic acid salt. Folding flexible phosphorescent material.
It realizes the preparation of high-efficiency phosphorescent materials in aqueous solution, has adjustable luminescence characteristics and long life, is suitable for information encryption and optoelectronic devices, and demonstrates the multi-level information encryption effect.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the synthesis of a class of aromatic bromine chains and ammonium salt compounds, the preparation of ammonium salt-doped polymer phosphorescent materials, and their applications in foldable flexible phosphorescent materials and information encryption. Background Art
[0002] Compared with inorganic phosphorescent materials, organic phosphorescent materials are easy to modify and adjust, have low toxicity and low price, which makes the development of organic room temperature phosphorescent (RTP) materials a research hotspot. At present, pure organic ultra-long room temperature phosphorescent materials have been widely used in information storage and encryption, bio-imaging, light-emitting devices, sensing and other fields. The general method to achieve organic ultra-long room temperature phosphorescence is to promote intersystem crossing (ISC) and suppress the non-radiative relaxation of triplet excitons, thereby increasing the phosphorescence lifetime. However, general organic luminophores are fat-soluble, which greatly limits their application in aqueous solutions. Therefore, it is very necessary to develop water-soluble and universal phosphors. Summary of the invention
[0003] The purpose of the present invention is to develop a general method for adjusting the luminescent color and lifespan by changing the luminescent core in order to solve the problem of poor water solubility of common phosphors. The method uses 4,4'-dihydroxybiphenyl and dibromopropane as reactants to reflux and purify the bromine chain product and react with trimethylamine to obtain an ammonium salt, and the ammonium salt is doped into PVA to obtain a simple phosphorescent polymer, and the luminescent color and lifespan are adjusted by changing the luminescent core, which has broad application prospects in the fields of information encryption, anti-counterfeiting and optoelectronic devices.
[0004] To achieve the above object, the present invention discloses the following technical solution: A class of aromatic cationic ammonium salt compounds characterized by including the following structure: (1) A class of aromatic compounds with bromine chains; (2) A class of aromatic cationic ammonium salt compounds:
[0005] in: (1) A method for synthesizing an aromatic compound with a bromine chain, characterized in that: Dissolve 4,4-dihydroxyterphenyl in a soluble solvent such as acetonitrile or acetone, N,N-dimethylformamide, dimethyl sulfoxide, methanol, ethanol, etc., add 1,3-dibromopropane and alkali, sodium carbonate, potassium carbonate or cesium carbonate, and heat under reflux for purification to obtain an aromatic compound with a bromine chain.
[0006] A class of aromatic cationic ammonium salt compounds characterized by having the following structure: (2) A method for synthesizing an aromatic ammonium salt compound, characterized in that: The bromine chain compound is dissolved in acetonitrile or acetone, N,N-dimethylformamide, dimethyl sulfoxide, methanol or ethanol soluble solvent, trimethylamine solution is added, and the mixture is heated to above 45° C. and reacted for 12-24 hours to obtain the product.
[0007] The present invention further discloses a type of phosphorescent polymer prepared by combining an aromatic ammonium salt compound with a polymer PVA. The preparation method thereof is as follows: firstly, the polymer PVA is dissolved in an appropriate amount of water, heated to 100°C and stirred for 2 hours to completely dissolve it, then the aromatic ammonium salt compound is dissolved in a small amount of water or methanol or ethanol, added to the stirred polymer PVA aqueous solution, mixed evenly, ultrasonicated, bubble-removed, spread on a glass plate, and dried to obtain the phosphorescent polymer.
[0008] The present invention further discloses a complex prepared from an aromatic ammonium salt compound and cucurbituril or cyclodextrin, which is characterized in that the ammonium salt compound and cucurbituril or cyclodextrin are weighed in proportion, the weighed solid is ground with water, and then a small amount of water is added to dissolve to obtain an aqueous solution of the complex. The weighed solid can also be directly added with water and ultrasonicated for at least half an hour to obtain an aqueous solution of the complex. It also includes a phosphorescent polymer prepared from a complex prepared from an aromatic ammonium salt compound and cucurbituril or cyclodextrin and a polymer PVA.
[0009] The present invention also discloses the application of a class of aromatic ammonium salt compounds and composites and polymer PVA in preparing phosphorescent polymers for preparing foldable flexible phosphorescent materials and information encryption. N-1 doped film is used to make flower stems and leaves (longest afterglow), and then N-5 doped film is used to make petals (second afterglow), and N-2 doped film is used to make the flower center (shortest afterglow). The experimental results show that: under 254 nm excitation, a "flower" pattern is displayed, and after removing the ultraviolet light excitation, within 1 second, the pattern is displayed as "petals" and "leaves", and after 3 seconds, only the "flower stem" and "leaves" with long afterglow are displayed.
[0010] A class of aromatic compounds with bromine chains, characterized by having the following structure:
[0011] The synthesis method of the bromine chain product is as follows: Dissolve the 4,4'-dihydroxy raw material and dibromopropane in acetone or acetonitrile, add potassium carbonate, stir and reflux overnight. After the reaction is completed, first remove the potassium carbonate by suction filtration, and wash the filter residue three times with dichloromethane, and collect the filtrate together to concentrate. Finally, there will be dibromopropane that cannot be dried, add a small amount of petroleum ether, precipitate solid, centrifuge, the solid is the crude product, and recrystallize or column chromatography to obtain the pure product.
[0012] Br-3 hydrogen spectrum: 1H NMR (400 MHz, CDCl3) δ 7.61 (s, 4H), 7.57 (d, J = 8.4 Hz,4H), 7.00 (d, J = 8.8 Hz, 4H), 4.16 (t, J = 6 Hz, 4H), 3.64 (t, J = 6.4 Hz,4H), 2.45 – 2.27 (m, 4H). Mass spectrum: m / z=504.0133 Br-2 hydrogen spectrum: 1 H NMR (400 MHz, CDCl3) δ 7.92 (d, J = 8.4 Hz, 4H), 7.73 (s, 2H), 7.09 (d, J = 8.8 Hz, 4H), 4.21 (t, J = 5.6 Hz, 4H), 3.65 (t, J = 6.4 Hz,4H), 2.43 – 2.32 (m, 4H). Mass spectrum: [M+H] + =560.9849 First, 1,3-dipropanol is reacted with p-toluenesulfonyl chloride to generate an OTs product, the OTs product is reacted with 2,2,4,4-tetrahydroxybiphenyl and potassium carbonate, etc., and purified by column chromatography to obtain an OH product, and the OH product is reacted with triphenylphosphine and carbon tetrabromide and purified by column chromatography to obtain a bromine chain product.
[0013] Br-1 H NMR spectrum data: 1 H NMR (400 MHz, CDCl3) δ 7.12 (d, J = 8.8 Hz, 2H), 6.56 – 6.52 (m, 4H), 4.14 (t, J = 5.6 Hz, 4H), 4.02 (t, J = 6 Hz, 4H), 3.64(t, J = 6.4 Hz, 4H), 3.38 (t, J = 6.4 Hz, 4H), 2.38 – 2.31 (m, 4H), 2.19 –2.12 (m, 4H). Mass spectrum: m / z=701.8826 A class of aromatic cationic ammonium salt compounds characterized by having the following structure:
[0014] The synthesis method of the ammonium salt product is as follows: The obtained pure bromine chain product is dissolved in acetonitrile or acetone, and trimethylamine solution is added to heat and react for about 24 hours. After the reaction is completed, the reaction solution is spin-dried and recrystallized to obtain a pure product.
[0015] N-1 hydrogen spectrum: 1 H NMR (400 MHz, D2O) δ 7.62 (d, J = 8.8 Hz, 4H), 7.10 (d, J =8.8 Hz, 4H), 4.21 (t, J = 5.6 Hz, 4H), 3.61 – 3.50 (m, 4H), 2.36 – 2.23 (m,4H). Mass spectrum: [M-Br] + =465.2107 N-2 Hydrogen Spectrum: 1 H NMR (400 MHz, CD3OD) δ 8.01 (d, J = 8.8 Hz, 4H), 7.83 (s,2H), 7.13 (d, J = 8.8 Hz, 4H), 4.23 (t, J = 5.6 Hz, 4H), 3.68 – 3.60 (m, 4H),3.23 (s, 4H), 2.42 – 2.31 (m, 4H).Mass spectrum: [M-2Br] 2+ =260.1421 N-3 hydrogen spectrum: 1 H NMR (400 MHz, DMSO) δ 7.12 (d, J = 8.4 Hz, 2H), 6.69 –6.60 (m, 4H), 4.08 (t, J = 5.6 Hz, 4H), 3.99 (t, J = 5.6 Hz, 4H), 3.58 – 3.50(m, 4H), 3.32 – 3.25 (m, 4H), 3.14 (s, 18H), 3.03 (s, 18H), 2.25 – 2.14 (m,4H), 2.08 – 1.97 (m, 4H).Mass spectrum: [M-Br] + =859.2555 N-4 hydrogen spectrum: 1H NMR (400 MHz, CD3OD) δ7.63 (s, 4H) 7.61 (d, J = 8.8 Hz,4H), 7.04 (d, J = 8.8 Hz , 4H), 4.18 (t, J = 5.6 Hz, 4H), 3.66–3.59 (m, 4H),3.22 (s, 18H), 2.38–2.29 (m, 4H).Mass spectrum: [M-Br] + =541.2429 N-5 hydrogen spectrum: 1 H NMR (400 MHz, CD3OD) δ 7.70 (d, J = 8.8 Hz, 2H), 7.25 (s,2H), 7.14 (d, J = 8.8 Hz, 2H), 4.22 (t, J = 5.6 Hz, 4H), 3.70 – 3.61 (m, 4H),3.22 (s, 18H), 2.40 – 2.30 (m, 4H).Mass spectrum: [M-Br] + =439.1958 Preparation of complexes of benzyl ammonium salt and cucurbituril or cyclodextrin: The ammonium salt compound and cucurbituril or cyclodextrin are weighed in proportion, the weighed solid can be ground first, added with two drops of water to dry, then added with two drops of water to dry, and then added with a small amount of water to dissolve to obtain an aqueous solution of the complex. Alternatively, the weighed solid can be directly added with water and ultrasonicated for at least half an hour to promote the host-guest interaction to obtain an aqueous solution of the complex. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 :1:1 NMR comparison of ammonium salt 1 and cucurbituril[7] complex (D2O, 298 K, 2 mmol) (I) object alone, (II) object + CB[7]; Figure 2 :1:1 NMR comparison of ammonium salt 1 and β-cyclodextrin complex (D2O, 298 K, 2 mmol) (I) guest alone, (II) guest + β-CD; Figure 3 : (I) fluorescence excitation (II) emission (III) phosphorescence lifetime (IV) fluorescence lifetime of ammonium salt N-1@PVA film; Figure 4 : Phosphorescent encrypted images. DETAILED DESCRIPTION The synthesis and application of the bromine chain and ammonium salt of the present invention are described in detail below in conjunction with the accompanying drawings, but the present invention is not limited to the following examples. In order to enable the public to have a full understanding of the present invention, the specific details are described in detail in the preferred embodiments of the present invention. The raw materials used in the present invention are all commercially available, and the unreported monomers are claimed for rights protection and disclosed preparation methods. This is hereby explained.
[0018] 1. Preparation method (1) Preparation of Br-1
[0019] Take 3.0 g of 2,4-dimethoxybromobenzene (CAS: 17715-69-4) and completely dissolve it in a 1,4-dioxane aqueous solution (1,4-dioxane: water = 4:1), then add 6.3 g of 2,4-dimethoxyphenylboric acid, 0.7 g of ferrocenedichloropalladium, and 5.9 g of sodium carbonate, and heat the mixed system to 95 ° C and reflux overnight. After the reaction is completed, the reaction solution is cooled to room temperature, the solvent is dried, dissolved in dichloromethane, and extracted with water three times. The organic layer is dried with anhydrous Na2SO4, and the sample is dried again, and M1 is separated by column chromatography.
[0020] Add M1 compound to a 100 mL round-bottom flask and dissolve it in dichloromethane. Add 20 equivalents of boron tribromide compound to the reaction system. After one day of reaction, drop the reaction solution into an ice-water mixture to precipitate a lavender powder, which is filtered to obtain the fully hydroxylated product M1-OH.
[0021] 1,3-dipropanol and sodium hydroxide were added to a 100 mL round-bottom flask and dissolved in tetrahydrofuran and water. 0.1 equivalent of p-toluenesulfonyl chloride was added to the reaction system. After reacting for 3 hours, the reaction solution was dropped into an ice-water mixture and extracted with dichloromethane three times. The organic layer was dried over anhydrous Na2SO4 and spin-dried to obtain the product OTs-OH.
[0022] Take 1g M1-OH and completely dissolve it in DMF, then add 10.6g OTs-OH, 19.0g potassium carbonate, 7.6g potassium iodide, and heat the mixed system to 160℃ and reflux for 24h. After the reaction, cool the reaction solution to room temperature, spin dry the solvent, dissolve it in dichloromethane, and extract it with water three times. Dry the organic layer with anhydrous Na2SO4, spin dry again, and separate it by column chromatography to obtain M1-3OH.
[0023] Take 0.5g M1-3OH and 2.3g triphenylphosphine and completely dissolve them in ultra-dry acetonitrile, add 8 equivalents of carbon tetrabromide into the reaction system, react for 6 hours, drop the reaction solution into a mixture of ice and water, filter to obtain a white solid, wash with a mixed solvent of methanol and water, and separate the remaining solid by column chromatography to obtain Br-1.
[0024] 1 H NMR (400 MHz, CDCl3) δ 7.12 (d, J = 8.8 Hz, 2H), 6.56 – 6.52 (m,4H), 4.14 (t, J = 5.6 Hz, 4H), 4.02 (t, J = 6 Hz, 4H), 3.64 (t, J = 6.4 Hz,4H), 3.38 (t, J = 6.4 Hz, 4H), 2.38 – 2.31 (m, 4H), 2.19 – 2.12 (m, 4H). Mass spectrum: m / z=701.8826 (2) Preparation of Br-2
[0025] Take 5g of 2,4-dimethoxybromobenzene (CAS: 15155-41-6) and completely dissolve it in a 1,4-dioxane aqueous solution (1,4-dioxane: water = 5:1), then add 6.3g of 4-hydroxyphenyl borate (CAS: 269409-70-3), 1.4g of triphenylphosphine palladium, and 7.1g of potassium carbonate, and heat the mixed system to 100°C and reflux overnight. After the reaction is completed, the reaction solution is cooled to room temperature, the solvent is dried by spin drying, dissolved in dichloromethane, and extracted with water three times. The organic layer is dried with anhydrous Na2SO4, and then spin dried again, and recrystallized to obtain M2-OH.
[0026] Take 3.0 g of M2-3OH and completely dissolve it in acetonitrile, then add 3.9 g of potassium carbonate, add 10 equivalents of 1,3-dibromopropane into the reaction system, heat to 85°C and reflux for 24 hours. After the reaction is completed, cool the reaction solution to room temperature, filter out the potassium carbonate, spin-dry the filtrate, and recrystallize to obtain Br-2.
[0027] 1 H NMR (400 MHz, CDCl3) δ 7.92 (d, J = 8.4 Hz, 4H), 7.73 (s, 2H), 7.09(d, J = 8.8 Hz, 4H), 4.21 (t, J = 5.6 Hz, 4H), 3.65 (t, J = 6.4 Hz, 4H), 2.43– 2.32 (m, 4H). Mass spectrum: [M+H] + =560.9849 (3) Preparation of Br-3
[0028] Take 3.0 g of 1,4-dibromobenzene (CAS: 106-37-6) and completely dissolve it in a 1,4-dioxane aqueous solution (1,4-dioxane: water = 5:1), then add 5.8 g of 2,4-dimethoxyphenylboronic acid, 1.0 g of tetrakistriphenylphosphine palladium, and 5.3 g of potassium carbonate, and heat the mixed system to 100 ° C and reflux overnight. After the reaction is completed, the reaction solution is cooled to room temperature, the solvent is dried, dissolved in dichloromethane, and extracted with water three times. The organic layer is dried with anhydrous Na2SO4, and the sample is dried again, and M3 is separated by column chromatography.
[0029] Add M3 compound to a 100 mL round-bottom flask and dissolve it in dichloromethane. Add 20 equivalents of boron tribromide compound to the reaction system. After reacting for 1 day, drop the reaction solution into an ice-water mixture to precipitate a lavender powder, which is filtered to obtain the fully hydroxylated product M3-OH.
[0030] Take 2.0 g of M3-3OH and completely dissolve it in acetonitrile, then add 4.2 g of potassium carbonate, add 20 equivalents of 1,3-dibromopropane into the reaction system, heat to 85°C and reflux for 24 hours. After the reaction is completed, cool the reaction solution to room temperature, filter out the potassium carbonate, spin-dry the filtrate, and recrystallize to obtain Br-3.
[0031] 1 H NMR (400 MHz, CDCl3) δ 7.61 (s, 4H), 7.57 (d, J = 8.4 Hz, 4H), 7.00(d, J = 8.8 Hz, 4H), 4.16 (t, J = 6 Hz, 4H), 3.64 (t, J = 6.4 Hz, 4H), 2.45 –2.27 (m, 4H). Mass spectrum: m / z=504.0133 (4) Preparation of N-1
[0032] First, according to the literature (B. Khan et al. Tetrahedron Letters ., 2015, 56 , 581–585.) Method for synthesizing N1-Br: 2.0 g N1-Br was dissolved in acetonitrile, 20 equivalents of trimethylamine were added, and the mixture was heated to 60 °C for reaction. After the reaction was completed, the solvent was dried and recrystallized to obtain N-1.
[0033] 1 H NMR (400 MHz, D2O) δ 7.62 (d, J = 8.8 Hz, 4H), 7.10 (d, J = 8.8 Hz,4H), 4.21 (t, J = 5.6 Hz, 4H), 3.61 – 3.50 (m, 4H), 2.36 – 2.23 (m, 4H). Mass spectrum: [M-Br] + =465.2107 (5) Preparation of N-2
[0034] Take 0.5 g of the previously synthesized Br-2 and completely dissolve it in acetonitrile, add 20 equivalents of trimethylamine, heat to 60°C for reaction, spin dry the solvent after the reaction is completed, and recrystallize to obtain N-2.
[0035] 1 H NMR (400 MHz, CD3OD) δ 8.01 (d, J = 8.8 Hz, 4H), 7.83 (s, 2H), 7.13(d, J = 8.8 Hz, 4H), 4.23 (t, J = 5.6 Hz, 4H), 3.68 – 3.60 (m, 4H), 3.23 (s,4H), 2.42 – 2.31 (m, 4H). Mass spectrum: [M-2Br] 2+ =260.1421 (6) Preparation of N-3
[0036] Take 0.5 g of the previously synthesized Br-1 and dissolve it in methanol, add 20 equivalents of trimethylamine, heat to 60°C for reaction, spin dry the solvent after the reaction is completed, and recrystallize to obtain N-3.
[0037] 1 H NMR (400 MHz, DMSO) δ 7.12 (d, J = 8.4 Hz, 2H), 6.69 – 6.60 (m,4H), 4.08 (t, J = 5.6 Hz, 4H), 3.99 (t, J= 5.6 Hz, 4H), 3.58 – 3.50 (m, 4H), 3.32 – 3.25 (m, 4H), 3.14 (s, 18H), 3.03 (s, 18H), 2.25 – 2.14 (m, 4H), 2.08– 1.97 (m, 4H).Mass spectrum: [M-Br] + =859.2555 (7) Preparation of N-4
[0038] Take 1.0 g of the previously synthesized Br-3 and dissolve it in acetonitrile, add 20 equivalents of trimethylamine, heat to 60°C for reaction, spin dry the solvent after the reaction is completed, and recrystallize to obtain N-4.
[0039] 1 H NMR (400 MHz, CD3OD) δ7.63 (s, 4H) 7.61 (d, J = 8.8 Hz, 4H), 7.04(d, J = 8.8 Hz , 4H), 4.18 (t, J = 5.6 Hz, 4H), 3.66–3.59 (m, 4H), 3.22 (s,18H), 2.38–2.29 (m, 4H). Mass spectrum: [M-Br] + =541.2429 (8) Preparation of N-5
[0040] First, according to the literature (SK Pradhan, et al. Synthesis ,.1971, p., 661 – 662) method to synthesize N5-Br: 2.0 g N1-Br was dissolved in acetonitrile, 20 equivalents of trimethylamine were added, and the mixture was heated to 60°C for reaction. After the reaction was completed, the solvent was dried and recrystallized to obtain N-5.
[0041] 1 H NMR (400 MHz, CD3OD) δ 7.70 (d, J = 8.8 Hz, 2H), 7.25 (s, 2H), 7.14(d, J = 8.8 Hz, 2H), 4.22 (t, J= 5.6 Hz, 4H), 3.70 – 3.61 (m, 4H), 3.22 (s,18H), 2.40 – 2.30 (m, 4H). Mass spectrum: [M-Br] + =439.1958. Example
[0042] Application of a class of aromatic ammonium salt compounds and their complexes with polymer PVA in the preparation of phosphorescent polymers: Luminescent materials are important research objects in the field of optoelectronics, and phosphorescent materials have great application prospects in encryption and anti-counterfeiting due to their large Stokes shift and long lifespan. Phosphorescent flexible polymer materials are more convenient for our application because of their easy preparation, foldability and good reproducibility. According to literature reports, polyvinyl alcohol (PVA) is a polymer matrix that can provide a rigid network. We doped the synthesized water-soluble cationic ammonium salt into PVA to obtain a phosphorescent polymer material with a long lifespan (1232ms) and high quantum yield (33.2%).
[0043] The preparation method is as follows: (1) First, weigh 1 g of polyvinyl alcohol solid into a 100 mL flask, add 20 mL of deionized water, heat to 100 °C, and reflux for 2-3 h. When the polyvinyl alcohol particles are completely dissolved and the solution in the flask becomes clear and transparent, stop heating and wait for it to cool to room temperature to obtain a 50 mg / mL polyvinyl alcohol solution.
[0044] (2) Prepare a doping material with a mass ratio of 1 wt%. Weigh 1.5 mg of ammonium salt solid, add about 0.5 mL of deionized water and ultrasonically dissolve it completely. Transfer it to a centrifuge tube containing 3 mL of polyvinyl alcohol solution, shake it slightly to initially mix it, and then ultrasonically mix it to make it more uniform and remove bubbles.
[0045] (3) Subsequently, the polymer organic film was prepared by drop coating: a glass slide was placed on a glass dish in a drying oven, and the solution was drawn from the centrifuge tube using a disposable rubber-tipped dropper and evenly dropped onto the glass slide until the entire glass slide was completely covered by the solution. After the drop coating was completed, the drying oven temperature was adjusted to 65 °C and the drying was continued for about 5 hours to completely dry the polymer film, and finally a polymer-based phosphorescent film was obtained.
[0046] The results show that the prepared phosphorescent polymer films are transparent and have good flexibility. They emit strong light under ultraviolet light and have a long afterglow after the light is turned off. They can be used to prepare foldable flexible phosphorescent materials and information encryption. Under 254nm excitation, a "flower" pattern is displayed. After the ultraviolet light excitation is removed, the pattern is displayed as "petals" and "leaves" within 1 second. After 3 seconds, only the "flower stem" and "leaves" with a long afterglow are displayed, realizing polymer-based multi-level information encryption.
Claims
1. A class of aromatic cationic ammonium salt compounds, Features Includes the following structure: (1) A class of aromatic compounds with bromine chains; (2) a class of aromatic cationic ammonium salt compounds; in: (1) A class of aromatic compounds with bromine chains ; (2) a class of aromatic cationic ammonium salt compounds; 。 2. A phosphorescent polymer prepared from the aromatic cationic ammonium salt compound described in claim 1 and polymer PVA.
3. A method for preparing a phosphorescent polymer by using the aromatic cationic ammonium salt compound of claim 2 and polymer PVA, Features: First, the polymer PVA is dissolved in an appropriate amount of water, heated at 100°C and stirred for 2 hours to completely dissolve it, then the aromatic ammonium salt compound is dissolved in a small amount of water or methanol or ethanol, added to the stirred polymer PVA aqueous solution, mixed evenly, ultrasonicated to remove bubbles, spread on a glass plate, and dried to obtain a phosphorescent polymer.
4. A complex of a phosphorescent polymer prepared from a class of aromatic cationic ammonium salt compounds as claimed in claim 1 and polymer PVA, and cucurbituril and cyclodextrin, Features: The ammonium salt compound and cucurbituril or cyclodextrin are weighed in proportion, the weighed solid is ground with water, and then a small amount of water is added to dissolve to obtain an aqueous solution of the complex; or the weighed solid is directly added with water and ultrasonicated for at least half an hour to obtain an aqueous solution of the complex.
5. A phosphorescent polymer prepared from a type of aromatic cationic ammonium salt compound as claimed in claim 4 and polymer PVA, a complex prepared from cucurbituril and cyclodextrin, and a phosphorescent polymer prepared from polymer PVA.
6. Application of the aromatic ammonium salt compound and its composite as claimed in claim 1 and polymer PVA in preparing phosphorescent polymers in foldable flexible phosphorescent materials and information encryption.