Preparation method of aluminum-niobium intermediate alloy for titanium alloy smelting

By adding rare earth elements in the preparation process of aluminum-niobium intermediate alloy and adopting specific process steps and devices, the problem of impurities generated during the processing of aluminum-niobium intermediate alloy is solved and its purity is improved.

CN118996189AInactive Publication Date: 2024-11-22CHINA NONFERROUS METALS HANGYE (BEIJING) NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096212.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The aluminum-niobium intermediate alloy used in the smelting of existing titanium alloys is prone to produce impurities during processing, affecting its purity.

Method used

During the preparation of aluminum-niobium intermediate alloy, rare earth elements are added and purity is improved by specific steps such as drying, mix pretreatment, ignition, insulation and slow cooling and slag gold separation.

Benefits of technology

It effectively reduces the impurity content in the aluminum-niobium intermediate alloy and improves its purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004988005580000011
    Figure HDA0004988005580000011
  • Figure HDA0004988005580000021
    Figure HDA0004988005580000021
  • Figure HDA0004988005580000031
    Figure HDA0004988005580000031
Patent Text Reader

Abstract

The invention provides a preparation method of an aluminum-niobium intermediate alloy for titanium alloy smelting. The preparation method comprises the following steps: raw material preparation: preparing a main raw material niobium pentoxide, a reducing agent metal aluminum powder, a slag former calcium oxide, rare earth, a heat supplementing agent and calcium fluoride, mixing and pretreating, adding the heat supplementing agent, igniting materials, preserving heat and slowly cooling, and separating slag from metal. According to the preparation method of the aluminum-niobium intermediate alloy for titanium alloy smelting, rare earth is added into raw materials of niobium pentoxide, metal aluminum powder serving as a reducing agent, calcium oxide serving as a slag former, a heat supplementing agent and calcium fluoride which are used in the aluminum-niobium intermediate alloy, and the aluminum-niobium intermediate alloy is prepared through mixing. By means of the method, impurities generated in the manufacturing process of the aluminum-niobium intermediate alloy can be reduced, and therefore the purity of the aluminum-niobium intermediate alloy is improved after the aluminum-niobium intermediate alloy is manufactured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of titanium alloys, and in particular to a method for preparing an aluminum-niobium master alloy used for smelting titanium alloys. Background Art

[0002] Titanium alloys are widely used in the aviation field due to their excellent comprehensive properties such as low density, high specific strength, high temperature resistance, corrosion resistance, and weldability.

[0003] In the production of titanium alloys, adding alloying elements can effectively improve certain properties of titanium alloys. However, since the added elements are affected by many factors such as density, melting point, distribution coefficient, and addition method, it is easy to cause segregation of uneven element distribution. At present, the method of intermediate alloys is generally used to solve the metallurgical defects caused by the above factors. As an intermediate alloy for titanium alloy production, since the birth of titanium alloy, it has been considered an important control factor and means to effectively improve the inhomogeneity of alloy components, produce high-quality titanium alloys, and improve material quality, and has received much attention from manufacturers.

[0004] The aluminum-niobium master alloy used in current titanium alloy smelting is made from niobium pentoxide, reducing agent aluminum powder, slag-forming agent calcium oxide and calcium fluoride. However, the aluminum-niobium master alloy made from the raw materials currently used is prone to produce impurities during the processing, which affects the purity of the aluminum-niobium master alloy.

[0005] Therefore, it is necessary to provide a method for preparing an aluminum-niobium master alloy for titanium alloy smelting to solve the above technical problems. Summary of the invention

[0006] The invention provides a method for preparing an aluminum-niobium master alloy for titanium alloy smelting, which solves the problem that the aluminum-niobium master alloy smelted from raw materials currently used is prone to produce impurities during processing, thereby affecting the purity of the aluminum-niobium master alloy.

[0007] In order to solve the above technical problems, the present invention provides a method for preparing an aluminum-niobium master alloy for titanium alloy smelting, comprising the following steps:

[0008] S1. Raw material preparation: prepare the main raw material niobium pentoxide, reducing agent metal aluminum powder, slag-making agent calcium oxide, rare earth, heat supplement and calcium fluoride;

[0009] S2. Mixing pretreatment: The raw materials in S1 are subjected to mixing pretreatment, the mixed material after batching is first dried at 80-120° C. for 1.0-3.0 h, and then mixed in a conical mixer for 1.5-3.0 h, and the filling rate in the mixer is 40.0%-65.0%;

[0010] S3, adding a heat supplement agent: putting the pretreated mixed material into a reaction device and adding a heat supplement agent at the same time;

[0011] S4, ignition material: ignite the material to cause thermite combustion reaction;

[0012] S5, heat preservation and slow cooling: After the reaction is completed, heat preservation and slow cooling are carried out at the original position for 1-3 hours, followed by natural cooling at room temperature;

[0013] S6. Slag-metal separation: After cooling, slag-metal separation is performed to obtain aluminum-niobium intermediate alloy, which is then cast.

[0014] Preferably, a casting device is required for casting the aluminum-niobium intermediate alloy in S6, the casting device includes a conveying frame, a fixing component is arranged on the surface of the conveying frame, the fixing component includes two slide rails, a plurality of sliding sleeves are sleeved on the surfaces of the two slide rails, a fixing seat is connected to the surface of the sliding sleeve, a casting mold body is arranged inside the plurality of fixing seats, a lifting device is arranged on the side of the conveying frame, a material discharge component is arranged above the lifting device, a rotating device is arranged above the material discharge component, and a heating device is arranged on one side of the rotating device.

[0015] Preferably, a fixing bolt is provided between the sliding sleeve and the sliding rail.

[0016] Preferably, the lifting device comprises a base, and a hydraulic telescopic rod is installed on the top of the base.

[0017] Preferably, the material discharge assembly comprises a material discharge hopper, the bottom of the material discharge hopper is connected to a material discharge pipe, a valve is arranged on the material discharge pipe, and a connecting frame is arranged on the surface of the material discharge hopper.

[0018] Preferably, the rotating device includes a hydraulic rod, the top end of the hydraulic rod is connected to a support frame, one end of the support frame is mounted with a motor, one end of the motor output shaft is fixedly connected to a rotating rod via a coupling, and the bottom end of the rotating rod is connected to a scraper.

[0019] Preferably, the heating device comprises a positioning frame, a surface of the positioning frame is provided with an annular air outlet pipe, and a surface of the annular air outlet pipe is provided with a plurality of air outlet holes.

[0020] Preferably, a fixing frame is provided on the surface of the positioning frame, a hot air blower is installed on the surface of the fixing frame, the input end and the output end of the hot air blower are both connected to a delivery pipe, and one end of one of the delivery pipes is connected to the annular air outlet pipe.

[0021] Preferably, a baffle is installed on one side of the surface of the conveying frame.

[0022] Preferably, a disassembly assembly is provided on one side of the connecting frame, and the disassembly assembly includes a disassembly seat, a mounting groove is opened on one side of the disassembly seat, a mounting block is provided inside the mounting groove, rubber pads are bonded to the top and bottom of the inner wall of the mounting groove, and a connecting piece is provided between the disassembly seat and the mounting block.

[0023] Compared with the related art, the preparation method of the aluminum-niobium master alloy for titanium alloy smelting provided by the present invention has the following beneficial effects:

[0024] The invention provides a method for preparing an aluminum-niobium master alloy for titanium alloy smelting. Rare earth is added to raw materials of niobium pentoxide, reducing agent metal aluminum powder, slag-forming agent calcium oxide, supplementary heat agent and calcium fluoride used in the aluminum-niobium master alloy, and the mixture is prepared. Impurities generated during the preparation of the aluminum-niobium master alloy can be reduced, thereby improving the purity of the aluminum-niobium master alloy after preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic structural diagram of a second embodiment of a method for preparing an aluminum-niobium master alloy for titanium alloy smelting provided by the present invention;

[0026] Figure 2 for Figure 1 An enlarged schematic diagram of part A is shown;

[0027] Figure 3 for Figure 1 An enlarged schematic diagram of part B is shown;

[0028] Figure 4 for Figure 1 A schematic diagram of the overall three-dimensional structure of the device shown;

[0029] Figure 5 A schematic structural diagram of a third embodiment of a method for preparing an aluminum-niobium master alloy for titanium alloy smelting provided by the present invention;

[0030] Figure 6 for Figure 5 An enlarged schematic diagram of part C is shown.

[0031] Numbers in the figure: 1. Conveyor rack,

[0032] 2. Fixing assembly, 21. Slide rail, 22. Slide sleeve, 23. Fixing seat, 24. Fixing bolt,

[0033] 3. Casting mold body,

[0034] 4. Lifting device, 41. Base, 42. Hydraulic telescopic rod,

[0035] 5. Feeding assembly, 51. Feeding hopper, 52. Feeding pipe, 53. Valve, 54. Connecting frame,

[0036] 6. Rotating device, 61. Hydraulic rod, 62. Support frame, 63. Motor, 64. Rotating rod, 65. Scraper,

[0037] 7. Heating device, 71. Positioning frame, 72. Annular air outlet pipe, 73. Air outlet hole, 74. Fixing frame, 75. Hot air blower, 76. Delivery pipe,

[0038] 8. Baffle,

[0039] 9. Disassembly assembly, 91. Disassembly seat, 92. Mounting groove, 93. Mounting block, 94. Rubber pad, 95. Connector. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with the accompanying drawings and implementation modes.

[0041] First embodiment

[0042] A method for preparing an aluminum-niobium master alloy for titanium alloy smelting comprises the following steps:

[0043] S1. Raw material preparation: prepare the main raw material niobium pentoxide, reducing agent metal aluminum powder, slag-making agent calcium oxide, rare earth, heat supplement and calcium fluoride;

[0044] S2. Mixing pretreatment: The raw materials in S1 are subjected to mixing pretreatment, the mixed material after batching is first dried at 80-120° C. for 1.0-3.0 h, and then mixed in a conical mixer for 1.5-3.0 h, and the filling rate in the mixer is 40.0%-65.0%;

[0045] S3, adding a heat supplement agent: putting the pretreated mixed material into a reaction device and adding a heat supplement agent at the same time;

[0046] S4, ignition material: ignite the material to cause thermite combustion reaction;

[0047] S5, heat preservation and slow cooling: After the reaction is completed, heat preservation and slow cooling are carried out at the original position for 1-3 hours, followed by natural cooling at room temperature;

[0048] S6. Slag-metal separation: After cooling, slag-metal separation is performed to obtain aluminum-niobium intermediate alloy, which is then cast.

[0049] Rare earths can also be replaced by inert gases: such as argon or helium, which can be used to protect the smelting process and reduce oxidation and the introduction of impurities.

[0050] Fluorides: such as calcium fluoride or aluminum fluoride, can react with impurities to form volatile substances, thereby removing impurities.

[0051] Chlorides: such as calcium chloride or aluminum chloride, can form low-melting-point chlorides with impurities during the smelting process, making them easier to remove.

[0052] Rare earth elements: Certain rare earth elements can be used as refining agents to improve the structure and properties of alloys.

[0053] Special compounds: Some specially designed compound refining agents combine multiple refining functions to improve the refining effect.

[0054] Compared with the related art, the preparation method of the aluminum-niobium master alloy for titanium alloy smelting provided by the present invention has the following beneficial effects:

[0055] The invention provides a method for preparing an aluminum-niobium master alloy for titanium alloy smelting. Rare earth is added to raw materials of niobium pentoxide, reducing agent metal aluminum powder, slag-forming agent calcium oxide, supplementary heat agent and calcium fluoride used in the aluminum-niobium master alloy, and the mixture is prepared. Impurities generated during the preparation of the aluminum-niobium master alloy can be reduced, thereby improving the purity of the aluminum-niobium master alloy after preparation.

[0056] Second embodiment

[0057] Please refer to Figure 1 , Figure 2 , Figure 3 and Figure 4 Based on the method for preparing an aluminum-niobium master alloy for titanium alloy smelting provided in the first embodiment of the present application, the second embodiment of the present application proposes another method for preparing an aluminum-niobium master alloy for titanium alloy smelting. The second embodiment is only a preferred embodiment of the first embodiment, and the implementation of the second embodiment will not affect the independent implementation of the first embodiment.

[0058] Specifically, the second embodiment of the present application provides a method for preparing an aluminum-niobium intermediate alloy for titanium alloy smelting. The difference is that, in a method for preparing an aluminum-niobium intermediate alloy for titanium alloy smelting, a casting device is required when casting the aluminum-niobium intermediate alloy in S6, and the casting device includes a conveying frame 1, and a fixing component 2 is arranged on the surface of the conveying frame 1. The fixing component 2 includes two slide rails 21, and the surfaces of the two slide rails 21 are both sleeved with a plurality of sliding sleeves 22, and the surfaces of the sliding sleeves 22 are connected to a fixing seat 23, and a casting mold body 3 is arranged inside the plurality of fixing seats 23, and a lifting device 4 is arranged on the side of the conveying frame 1, and a material discharge component 5 is arranged above the lifting device 4, and a rotating device 6 is arranged above the material discharge component 5, and a heating device 7 is arranged on one side of the rotating device 6.

[0059] Two slide rails 21 are symmetrically connected to the surface of the conveyor frame 1. The slide rails 21 are made of rubber and can rotate with the conveyor frame 1. The conveyor frame 1 is driven by a driving motor. The use of the slide rails 21 and the sliding sleeves 22 can adjust the position of the fixed seat 23. When the position of the fixed seat 23 is adjusted, the sliding sleeve 22 is driven to move on the surface of the slide rails 21 by pulling the fixed seat 23. When the fixed seat 23 moves to a suitable position, the fixing bolt 24 is used to pass through the sliding sleeve 22 and connect with the slide rail 21.

[0060] A fixing bolt 24 is disposed between the sliding sleeve 22 and the sliding rail 21 .

[0061] The lifting device 4 includes a base 41 , and a hydraulic telescopic rod 42 is installed on the top of the base 41 .

[0062] The base 41 is connected to the side of the conveying frame 1, and the use of the hydraulic telescopic rod 42 can adjust the upper and lower positions of the unloading component 5. The connecting frame 54 is connected to the top of the hydraulic telescopic rod 42. The use of the unloading pipe 52 can be connected to the casting mold body 3 to unload the casting liquid. The use of the valve 53 can operate the switch of the unloading pipe 52. When in use, when pouring the inside of the casting mold body 3, first start the hydraulic telescopic rod 42 to drive the unloading hopper 51 to move downward through the connecting frame 54. When the unloading hopper 51 moves downward, it drives the unloading pipe 52 at the bottom to move to connect with the casting mold body 3. After the unloading pipe is connected to the casting mold body 3, stop the work of the hydraulic telescopic rod 42, and then open the valve 53 on the surface of the unloading pipe 52 to transport the liquid inside the unloading hopper 51 to the inside of the casting mold body 3 through the unloading pipe 52.

[0063] The material discharge assembly 5 comprises a material discharge hopper 51 , the bottom of which is connected to a material discharge pipe 52 , a valve 53 is provided on the material discharge pipe 52 , and a connecting frame 54 is provided on the surface of the material discharge hopper 51 .

[0064] The rotating device 6 includes a hydraulic rod 61, the top end of the hydraulic rod 61 is connected to a support frame 62, one end of the support frame 62 is installed with a motor 63, one end of the output shaft of the motor 63 is fixedly connected to a rotating rod 64 through a coupling, and the bottom end of the rotating rod 64 is connected to a scraper 65.

[0065] The hydraulic rod 61 is installed on the surface of the connecting frame 54 through the rotating shaft. The use of the hydraulic rod 61 can drive the scraper 65 to move to the inside of the lower hopper 51 and fit with it. The use of the motor 63 can drive the scraper 65 to rotate inside the lower hopper 51. The positioning frame 71 is installed on the surface of the rotating rod 64. The use of the heating device 7 can melt the residue remaining on the inner wall of the lower hopper 51 to facilitate the scraping of the scraper 65. When in use, first drive the scraper 65 to rotate to the top of the lower hopper 51 through the hydraulic rod 61. When the scraper 65 rotates to the top of the lower hopper 51, start the hydraulic rod 61 to drive the scraper 65 to move to the bottom of the hopper. 51 contacts the inner wall of the lower hopper 51. When the scraper 65 moves to contact the inner wall of the lower hopper 51, the hydraulic rod 61 is stopped, and then the motor 63 is started to drive the scraper 65 to rotate inside the lower hopper 51 through the rotating rod 64. When the scraper 65 rotates inside the lower hopper 51, the hot air blower 75 is started to convey the hot air to the inside of the annular air outlet pipe 72 through the conveying pipe 76. After the hot air is conveyed to the inside of the annular air outlet pipe 72, it is blown to the inner wall of the lower hopper 51 through the multiple air outlet holes 73 on the surface of the annular air outlet pipe 72 to melt the residue. At the same time, the scraper 65 can clean the residue on the inner wall of the lower hopper 51.

[0066] The heating device 7 comprises a positioning frame 71 , a surface of which is provided with an annular air outlet pipe 72 , and a surface of which is provided with a plurality of air outlet holes 73 .

[0067] A fixing frame 74 is disposed on the surface of the positioning frame 71 , and a hot air blower 75 is installed on the surface of the fixing frame 74 . The input end and the output end of the hot air blower 75 are both connected to a delivery pipe 76 , and one end of one of the delivery pipes 76 is connected to the annular air outlet pipe 72 .

[0068] A baffle 8 is installed on one side of the surface of the conveying frame 1 .

[0069] Compared with the related art, the preparation method of the aluminum-niobium master alloy for titanium alloy smelting provided by the present invention has the following beneficial effects:

[0070] The present invention provides a method for preparing an aluminum-niobium intermediate alloy for titanium alloy smelting. A conveyor frame 1 is provided with two slide rails 21, a plurality of slide sleeves 22 with fixed seats 23, and a material discharge assembly 5. When liquid is poured into a casting mold body 3 of different sizes, the position of the fixed seat 23 can be adjusted. A heating device 7 is provided on the surface of a rotating rod 64 for use with a scraper 65, which can facilitate cleaning of impurities remaining on the inner wall of the material discharge hopper 51.

[0071] Third embodiment

[0072] Please refer to Figure 5 and Figure 6Based on the method for preparing an aluminum-niobium master alloy for titanium alloy smelting provided in the first embodiment of the present application, the third embodiment of the present application proposes another method for preparing an aluminum-niobium master alloy for titanium alloy smelting. The third embodiment is only a preferred embodiment of the first embodiment, and the implementation of the third embodiment will not affect the independent implementation of the first embodiment.

[0073] Specifically, the difference of the method for preparing an aluminum-niobium intermediate alloy for titanium alloy smelting provided in the third embodiment of the present application is that, in a method for preparing an aluminum-niobium intermediate alloy for titanium alloy smelting, a disassembly component 9 is provided on one side of the connecting frame 54, and the disassembly component 9 includes a disassembly seat 91, and a mounting groove 92 is opened on one side of the disassembly seat 91, and a mounting block 93 is provided inside the mounting groove 92, and rubber pads 94 are bonded to the top and bottom of the inner wall of the mounting groove 92, and a connecting piece 95 is provided between the disassembly seat 91 and the mounting block 93.

[0074] The disassembly seat 91 is connected to the top end of the hydraulic telescopic rod 42, one end of the mounting block 93 is connected to one end of the connecting frame 54, the use of the rubber pad 94 can play a squeezing role when the mounting block 93 is installed inside the mounting groove 92, and a connecting hole compatible with the connecting piece 95 is opened between the disassembly seat 91 and the mounting block 93.

[0075] The working principle of the method for preparing an aluminum-niobium master alloy for titanium alloy smelting provided by the present invention is as follows:

[0076] During use, when the lower hopper 51 is disassembled and replaced, first take out the connecting piece 95 between the connecting frame 54 and the disassembly seat 91. After the connecting piece 95 is taken out, the connecting frame 54 is moved to one side by pulling the lower hopper 51. When the connecting frame 54 moves, it drives the mounting block 93 to separate from the mounting groove 92.

[0077] Compared with the related art, the preparation method of the aluminum-niobium master alloy for titanium alloy smelting provided by the present invention has the following beneficial effects:

[0078] The present invention provides a method for preparing an aluminum-niobium master alloy for titanium alloy smelting. A disassembly assembly 9 is arranged on one side of a connecting frame 54 so that a damaged lower hopper 51 can be disassembled and replaced after the lower hopper 5 is used for a long time.

[0079] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing an aluminum-niobium master alloy for titanium alloy smelting, characterized in that: The following steps are involved: S1. Raw material preparation: prepare the main raw material niobium pentoxide, reducing agent metal aluminum powder, slag-making agent calcium oxide, rare earth, heat supplement and calcium fluoride; S2. Mixing pretreatment: The raw materials in S1 are subjected to mixing pretreatment, the mixed material after batching is first dried at 80-120° C. for 1.0-3.0 h, and then mixed in a conical mixer for 1.5-3.0 h, and the filling rate in the mixer is 40.0%-65.0%; S3, adding a heat supplement agent: putting the pretreated mixed material into a reaction device and adding a heat supplement agent at the same time; S4, ignition material: ignite the material to cause thermite combustion reaction; S5, heat preservation and slow cooling: After the reaction is completed, heat preservation and slow cooling are carried out at the original position for 1-3 hours, followed by natural cooling at room temperature; S6. Slag-metal separation: After cooling, slag-metal separation is performed to obtain aluminum-niobium intermediate alloy, which is then cast.

2. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 1, characterized in that: When casting the aluminum-niobium master alloy in S6, a casting device is required, the casting device includes a conveying frame, a fixing component is arranged on the surface of the conveying frame, the fixing component includes two slide rails, a plurality of sliding sleeves are sleeved on the surfaces of the two slide rails, a fixing seat is connected to the surface of the sliding sleeve, a casting mold body is arranged inside the plurality of fixing seats, a lifting device is arranged on the side of the conveying frame, a material discharge component is arranged above the lifting device, a rotating device is arranged above the material discharge component, and a heating device is arranged on one side of the rotating device.

3. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 2, characterized in that: A fixing bolt is arranged between the sliding sleeve and the sliding rail.

4. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 2, characterized in that: The lifting device comprises a base, and a hydraulic telescopic rod is installed on the top of the base.

5. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 2, characterized in that: The material discharge assembly comprises a material discharge hopper, the bottom of the material discharge hopper is connected with a material discharge pipe, a valve is arranged on the material discharge pipe, and a connecting frame is arranged on the surface of the material discharge hopper.

6. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 2, characterized in that: The rotating device comprises a hydraulic rod, the top end of which is connected to a support frame, one end of which is mounted with a motor, one end of the motor output shaft is fixedly connected to a rotating rod via a coupling, and the bottom end of the rotating rod is connected with a scraper.

7. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 2, characterized in that: The heating device comprises a positioning frame, a surface of the positioning frame is provided with an annular air outlet pipe, and a surface of the annular air outlet pipe is provided with a plurality of air outlet holes.

8. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 7, characterized in that: A fixing frame is arranged on the surface of the positioning frame, a hot air blower is installed on the surface of the fixing frame, the input end and the output end of the hot air blower are both connected with a delivery pipe, and one end of one of the delivery pipes is connected to the annular air outlet pipe.

9. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 2, characterized in that: A baffle is installed on one side of the conveying frame surface.

10. The method for preparing an aluminum-niobium master alloy for titanium alloy smelting according to claim 5, characterized in that: A disassembly assembly is provided on one side of the connecting frame, and the disassembly assembly includes a disassembly seat, a mounting groove is opened on one side of the disassembly seat, a mounting block is provided inside the mounting groove, rubber pads are bonded to the top and bottom of the inner wall of the mounting groove, and a connecting piece is provided between the disassembly seat and the mounting block.