Method for rapidly preparing compact aluminum phosphate ceramic at low temperature

By adding yttrium oxide powder to aluminum phosphate powder and using discharge plasma sintering technology, the problems of long sintering time and low density of dense aluminum phosphate ceramics are solved, and the rapid preparation of dense ceramics is achieved at low temperature, with rapid sintering, energy-saving and environmentally friendly Features: suitable for the production of complex shape ceramics and improve its application potential in the fields of heat insulation and wave transmission.

CN119038983AActive Publication Date: 2024-11-29ZHENGZHOU UNIV

Patent Information

Application Number
CN202410935105.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-29
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

In the prior art, dense aluminum phosphate ceramics have a long sintering time and low density, which limits their application in the fields of heat insulation and wave transmission.

Method used

Using discharge plasma sintering technology, 3-6 wt.% sintering additive yttrium oxide powder is added to the aluminum phosphate powder, and dry mixing is performed using an acoustic resonance mixer, and then discharge plasma is performed in a graphite mold. Sintering, controlling the heating rate and pressure, and preparing dense aluminum phosphate ceramics.

Benefits of technology

It realizes the rapid preparation of dense aluminum phosphate ceramics at low temperatures, with fast cooling rate, short sintering time, energy-saving and environmentally friendly characteristics, and has a relative density of 97%. It is suitable for the production of ceramic products with complex shapes and high dimensional accuracy, which broadens its wave-transmitting conditions. , application in the field of thermal insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038983A_ABST
    Figure CN119038983A_ABST
Patent Text Reader

Abstract

The invention provides a method for rapidly preparing compact aluminum phosphate ceramic at low temperature, which comprises the following steps: respectively weighing aluminum phosphate powder and 3-6wt.% of sintering aid yttrium oxide powder, and carrying out dry mixing and uniform mixing by using an acoustic resonance mixer to obtain primarily mixed powder; sieving the obtained primarily mixed powder with a 200-mesh sieve to obtain mixed powder; and putting the mixed powder into a graphite mold, and sintering the graphite mold in a discharge plasma sintering furnace to obtain the compact aluminum phosphate ceramic. The problem that the aluminum phosphate ceramic is difficult to sinter is solved by adding a small amount of sintering aid, low-temperature rapid densification of the aluminum phosphate ceramic is realized by combining a discharge plasma sintering technology, and the relative density of the compact aluminum phosphate ceramic prepared by the method can reach 97%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic materials, and in particular to a method for rapidly preparing dense aluminum phosphate ceramics at low temperature. Background Art

[0002] Spark plasma sintering (SPS) has the characteristics of fast heating and cooling rates, high heat transfer efficiency and short sintering time. It can be used to prepare a variety of materials such as intermetallic compounds, structural and functional ceramics, and is a popular sintering technology in recent years. SPS mainly generates plasma by applying pulse current to the powder, causing discharge between powder particles, thereby generating Joule heat and forming local high temperature; at the same time, under the action of external pressure, the powder particles are compressed to promote mass transfer and sintering process. Therefore, compared with traditional sintering methods, SPS technology has greater advantages in ceramic densification. Ceramics prepared using this technology usually have the characteristics of dense organization and uniform structure.

[0003] Aluminum phosphate ceramics are resistant to high temperatures and have excellent thermal stability and wave transmission properties. They have good application prospects in the fields of heat insulation, wave transmission, catalysis, etc. However, due to the difficulty in sintering aluminum phosphate materials, there are relatively few studies on dense aluminum phosphate ceramics, and most of them use pressureless sintering to prepare phosphate-based materials, which has the problems of long sintering time and relatively low density. Therefore, it is very necessary to develop a method for quickly preparing dense aluminum phosphate ceramics to broaden its application in the fields of heat insulation, wave transmission, etc. Summary of the invention

[0004] Based on the above technical problems, the present invention proposes a method for rapidly preparing dense aluminum phosphate ceramics at low temperature.

[0005] A method for rapidly preparing dense aluminum phosphate ceramics at low temperature, the method comprising the following steps: S1. Weigh aluminum phosphate powder and 3-6 wt.% of yttrium oxide powder as a sintering aid respectively, and use an acoustic resonance mixer to dry-blend and mix them evenly to obtain a primary mixed powder; S2, passing the obtained primary mixed powder through a 200-mesh sieve to obtain a mixed powder; S3, loading the mixed powder into a graphite mold and placing it in a spark plasma sintering furnace for sintering to obtain dense aluminum phosphate ceramics.

[0006] Preferably, in step S1, the acoustic resonance mixer is a MixBox-G1, and the process parameters of mixing the raw materials by the acoustic resonance mixer are as follows: the mixing container is an acrylic mixing tank, the program control mode is an automatic mode, the mixing acceleration is 30-60 g, the vibration frequency is 60 Hz~66 Hz, and the vibration time is 5-10 min.

[0007] Preferably, in step S3, the spark plasma sintering atmosphere is a vacuum atmosphere, the temperature is 1000-1100° C., the time is 5-10 min, and the pressure is 30 MPa.

[0008] Preferably, the heating rate of spark plasma sintering is controlled as follows: the heating rate is 50°C / min in the range of room temperature to 700°C; the heating rate is 40°C / min in the range of 700°C to 1000-1100°C.

[0009] Beneficial effects: (1) The present invention provides a method for rapidly preparing dense aluminum phosphate ceramics at low temperature, by adding a small amount of yttrium oxide powder as a sintering aid and adopting a spark plasma sintering technology to prepare dense ceramics, which has the characteristics of fast heating and cooling rate, short sintering time, and energy saving and environmental protection; (1) The method for rapidly preparing dense aluminum phosphate ceramics at low temperature provided by the present invention has a simple process and a short production cycle. Graphite molds of different shapes and sizes can be designed according to actual application requirements for loading and sintering, and are suitable for producing ceramic products with complex shapes and high dimensional accuracy requirements; (3) The dense aluminum phosphate ceramic prepared by the present invention has uniform phase distribution, and the particles are tightly bound together. Its relative density reaches 97%, and it is expected to be widely used in the fields of wave transmission and heat insulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 The XRD pattern of the aluminum phosphate ceramics prepared in Example 1-3; Figure 2 This is the SEM image of the dense aluminum phosphate ceramic prepared in Example 2. DETAILED DESCRIPTION

[0011] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0012] In the following comparative examples and embodiments: Acoustic resonance mixer: MixBox-G1 acoustic resonance mixer; Embodiment 1 A method for rapidly preparing dense aluminum phosphate ceramics at low temperature, the steps of the method are as follows: S1. Weigh 4 g of aluminum phosphate powder and 0.12 g of sintering aid yttrium oxide powder respectively, use an acoustic resonance mixer to dry-blend and mix them evenly to obtain a primary mixed powder; The process parameters of mixing raw materials with the acoustic resonance mixer are as follows: the mixing container is an acrylic mixing tank, the program control mode is automatic mode, the mixing acceleration is 30 g, the vibration frequency is 63.1 Hz, and the vibration time is 5 min.

[0013] S2, passing the obtained primary mixed powder through a 200-mesh sieve to obtain a mixed powder; S3. Load the mixed powder into a graphite mold with an inner diameter of 30 mm and place it in a spark plasma sintering furnace. After vacuuming, run the program for sintering. First, heat it to 700 °C at a rate of 50 °C / min, and then heat it to the sintering temperature of 1100 °C at a rate of 40 °C / min. At this time, the axial pressure is 30 MPa. Keep warm for 10 min, take out the sample after cooling, and obtain dense aluminum phosphate ceramics.

[0014] Embodiment 2 A method for rapidly preparing dense aluminum phosphate ceramics at low temperature, the steps of the method are as follows: S1. Weigh 4 g of aluminum phosphate powder and 0.24 g of sintering aid yttrium oxide powder respectively, use an acoustic resonance mixer to dry mix and mix evenly to obtain a primary mixed powder; The process parameters of mixing raw materials with the acoustic resonance mixer are as follows: the mixing container is an acrylic mixing tank, the program control mode is automatic mode, the mixing acceleration is 30 g, the vibration frequency is 63.1 Hz, and the vibration time is 5 min.

[0015] S2, passing the obtained primary mixed powder through a 200-mesh sieve to obtain a mixed powder; S3. Load the mixed powder into a graphite mold with an inner diameter of 30 mm and place it in a spark plasma sintering furnace. After vacuuming, run the program for sintering. First, heat it to 700 °C at a rate of 50 °C / min, and then heat it to the sintering temperature of 1100 °C at a rate of 40 °C / min. At this time, the axial pressure is 30 MPa. Keep warm for 10 min, take out the sample after cooling, and obtain dense aluminum phosphate ceramics.

[0016] Embodiment 3 A method for rapidly preparing dense aluminum phosphate ceramics at low temperature, the steps of the method are as follows: S1. Weigh 4 g of aluminum phosphate powder and 0.12 g of sintering aid yttrium oxide powder respectively, use an acoustic resonance mixer to dry-blend and mix them evenly to obtain a primary mixed powder; The process parameters of mixing raw materials with the acoustic resonance mixer are as follows: the mixing container is an acrylic mixing tank, the program control mode is automatic mode, the mixing acceleration is 30 g, the vibration frequency is 63.1 Hz, and the vibration time is 5 min.

[0017] S2, passing the obtained primary mixed powder through a 200-mesh sieve to obtain a mixed powder; S3. Load the mixed powder into a graphite mold with an inner diameter of 30 mm and place it in a spark plasma sintering furnace. After vacuuming, run the program for sintering. First, heat it to 700 °C at a rate of 50 °C / min, and then heat it to a sintering temperature of 1000 °C at a rate of 40 °C / min. At this time, the axial pressure is 30 MPa. Keep warm for 10 min, take out the sample after cooling, and obtain a dense aluminum phosphate ceramic.

[0018] Comparative Example 1 A method for rapidly preparing dense aluminum phosphate ceramics at low temperature, the steps of the method are as follows: S1. Weigh 4 g of aluminum phosphate powder and 0.24 g of sintering aid yttrium oxide powder respectively, use an acoustic resonance mixer to dry mix and mix evenly to obtain a primary mixed powder; The process parameters of mixing raw materials with the acoustic resonance mixer are as follows: the mixing container is an acrylic mixing tank, the program control mode is automatic mode, the mixing acceleration is 30 g, the vibration frequency is 63.1 Hz, and the vibration time is 5 min.

[0019] S2, passing the obtained primary mixed powder through a 200-mesh sieve to obtain a mixed powder; S3. The mixed powder is pre-pressed into a ceramic block with a diameter of 30 mm, placed in a box furnace at 1100 °C for pressureless sintering, and the temperature is raised to 1100 °C at a rate of 2 °C / min. The temperature is kept at this temperature for 2 h, and the sample is taken out after cooling to obtain aluminum phosphate ceramics.

[0020] The aluminum phosphate ceramics prepared in Examples 1-3 were characterized by X-ray diffraction (XRD). Figure 1 Shown: From Figure 1 It can be seen that a small amount of aluminum metaphosphate exists in the aluminum phosphate ceramic phase prepared by adding 3wt.% sintering aid, while the aluminum phosphate ceramic prepared by adding 6wt.% sintering aid does not contain any impurities in the XRD spectrum, indicating that single-phase aluminum phosphate ceramics can be prepared by this method.

[0021] The microstructure of the aluminum phosphate ceramic prepared in Example 2 was tested using a scanning electron microscope (SEM). The results are as follows: Figure 2 Shown: From Figure 2 It can be seen that the prepared aluminum phosphate ceramic particles are tightly combined and evenly distributed, indicating that the aluminum phosphate ceramics prepared by the method provided by the present invention are relatively dense.

[0022] It has been determined that the relative densities of the samples obtained in Examples 1-3 and Comparative Example 1 are 97.0%, 97.4%, 80.1% and 65.4%, respectively, which indicates that compared with pressureless sintering, the aluminum phosphate ceramics prepared by SPS technology at 1100°C and 1000°C have higher relative densities than those prepared by pressureless sintering, and are increased by 49% and 23%, respectively, further illustrating that the method provided by the present invention can achieve low-temperature rapid densification of aluminum phosphate ceramics.

[0023] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for rapidly preparing dense aluminum phosphate ceramics at low temperature, characterized in that: The steps of the method are as follows: S1. Weigh aluminum phosphate powder and 3-6 wt.% of yttrium oxide powder as a sintering aid respectively, and use an acoustic resonance mixer to dry-blend and mix them evenly to obtain a primary mixed powder; S2, passing the obtained primary mixed powder through a 200-mesh sieve to obtain a mixed powder; S3, loading the mixed powder into a graphite mold and placing it in a spark plasma sintering furnace for sintering to obtain dense aluminum phosphate ceramics.

2. The method for rapidly preparing dense aluminum phosphate ceramics at low temperature according to claim 1, characterized in that: In step S1, the acoustic resonance mixer is a MixBox-G1, and the process parameters of mixing raw materials by the acoustic resonance mixer are as follows: the mixing container is an acrylic mixing tank, the program control mode is an automatic mode, the mixing acceleration is 30-60 g, the vibration frequency is 60 Hz~66 Hz, and the vibration time is 5-10 min.

3. The method for rapidly preparing dense aluminum phosphate ceramics at low temperature according to claim 1, characterized in that: In step S3, the spark plasma sintering is performed in a vacuum atmosphere, at a temperature of 1000-1100°C, for 5-10 min, and at a pressure of 30 MPa.

4. The method for rapidly preparing dense aluminum phosphate ceramics at low temperature according to claim 3, characterized in that: The heating rate of spark plasma sintering is controlled as follows: the heating rate is 50°C / min in the range of room temperature to 700°C; the heating rate is 40°C / min in the range of 700°C to 1000-1100°C.

Citation Information

Patent Citations

  • Aluminum phosphate material and preparation method thereof

    CN115504445A

  • High-entropy tetraboride / hexaboride material and preparation method thereof

    CN117865685A

  • Process for preparing biological ceramic material of transparent bata-tricalcium phosphate and application thereof

    CN1793022A

  • Sintering method of calcium phosphate ceramic material

    JP1998251057A

  • Calcium phosphate-based ceramic sintered article and its production

    JP2000335962A

Cited By

  • Method for preparing compact aluminum phosphate ceramic at ultralow temperature based on zinc oxide-boric acid synergistic fluxing

    CN122212720A

  • A method for preparing a phosphate ceramic material which can be prepared at low temperature and served at high temperature

    CN122725827A