Preparation method of molybdenum-based alloy high-temperature protective coating

By optimizing the embedding and seepage method and high-temperature short-time heat treatment, the existing coating is solved for the sensitivity of the molybdenum-based alloy composition and tissue characteristics, and the preparation of high-temperature protective coatings with a wide range of application and low cost is achieved, which significantly improves the molybdenum-based coating. The high temperature oxidation resistance of the alloy.

CN119040800APending Publication Date: 2024-11-29TIANMUSHAN LABORATORY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411161789.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The antioxidant coating prepared by the existing embedding and permeability method is sensitive to the composition and structure characteristics of molybdenum-based alloys, and cannot be applied to molybdenum-based alloys of various alloy components and complex shapes. The process is complex and the cost is high, making it difficult to achieve high efficiency and high performance. Preparation of high temperature protective coating.

Method used

Based on the conventional embedding and permeability method, the time, temperature and powder composition are optimized, combined with high-temperature short-term heat treatment, and high-temperature protective coating with low residual stress and tight bonding to the matrix is ​​prepared. It is suitable for pure molybdenum, TZM alloys and complex shape molybdenum Base alloy.

Benefits of technology

It realizes a wide range of application, simple process and low-cost high-temperature protective coating preparation, significantly improves the high-temperature anti-oxidation performance of molybdenum-based alloys, reduces the preparation cost and time, and is suitable for molybdenum-based coatings containing carbide and oxide particles. Composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040800A_ABST
    Figure CN119040800A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of design and preparation of refractory alloy thermal protection coatings. The preparation method of the molybdenum-based alloy high-temperature protective coating comprises the steps that a coated substrate is pretreated, Si, B and NaF powder are subjected to ball milling, Al2O3 powder is added and mixed to be uniform, the alloy is buried into the mixed powder to be subjected to embedding infiltration treatment, the temperature ranges from 900 DEG C to 1300 DEG C, the heating rate ranges from 10 DEG C / min to 30 DEG C / min, and the heat preservation time ranges from 10 hrs to 50 hrs; according to the method, the time, the temperature, the powder components and other parameters used in the embedding infiltration process are optimized, meanwhile, the high-temperature and short-time heat treatment is carried out on the coating obtained after embedding infiltration treatment, and therefore the heat conductivity of the coating is improved, and the service life of the coating is prolonged. The prepared coating is small in residual stress, tightly combined with a matrix and excellent in high-temperature protection performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of design and preparation of refractory alloy thermal protective coatings. More specifically, it relates to a method of preparing a high-temperature anti-oxidation coating that is uniform, dense and tightly bonded to a substrate by performing embedding infiltration treatment on a molybdenum-based alloy and subsequent heat treatment. Background Art

[0002] Molybdenum (Mo)-based alloys can be used to make various high-temperature and ultra-high-temperature structural parts due to their advantages such as high melting point, low thermal expansion coefficient, and excellent high-temperature mechanical properties. They have a broad application market in the fields of aerospace, nuclear industry, machinery, etc. However, molybdenum-based alloys will suffer from severe oxidative corrosion in medium and high temperature oxidizing environments, affecting their service performance. This is because the main oxidation products of molybdenum-based alloys are glassy silicon dioxide (SiO2) and molybdenum oxide (MoO3). Molybdenum oxide will volatilize rapidly when the temperature reaches 600°C and above, forming a large number of holes in the oxide layer of silicon dioxide, causing oxidative corrosion to continue to proceed into the interior of the alloy. At present, researchers at home and abroad mostly use the method of adding alloying elements or preparing antioxidant coatings to improve the oxidation resistance of molybdenum-based alloys. The coating prepared by laser cladding technology has better effect, but the preparation process is complicated, the cost is high, and the matching degree of thermal expansion coefficient between the substrate and the coating is extremely high; the coating prepared by diffusion infiltration has good bonding with the substrate, and the process is simple and low-priced, but this method is more suitable for pure molybdenum or molybdenum-based alloys with low alloying degree, and the high-temperature protection effect is poor for molybdenum-based alloys with more complex composition and microstructure.

[0003] In the invention patent CN116837376A "A method for preparing a modified MoSi2 anti-oxidation coating on the surface of molybdenum or molybdenum alloy", Wang Li and others prepared a MoSi2-TiNbVZrAl composite coating on the surface of molybdenum or molybdenum alloy by laser cladding process. The composite coating has good anti-oxidation performance, good density and bonding performance with the substrate. However, the preparation process of this coating involves laser cladding process, mechanical alloying of powder, gas atomization method and other preparation methods. The process is complicated, the steps are numerous, the equipment and technical conditions are extremely high, and the cost is high. In addition, the above coating preparation method is difficult to apply to components with complex shapes.

[0004] Invention patent CN108118340A "Mo5Si3-MoSi2-SiO2 high temperature protective composite coating on the surface of molybdenum and molybdenum alloy electrodes and preparation method" proposes a method for preparing coatings on the surface of molybdenum and molybdenum alloy electrodes by combining vacuum activated infiltration with high temperature oxidation process. First, the Mo5Si3-MoSi2 composite coating is obtained by embedding infiltration, and then a continuous and dense SiO2 coating is obtained on the surface of MoSi2 by high temperature oxidation process. This preparation method is simple, the coating has an anti-oxidation life of 250 hours at 1600°C, and has excellent high temperature protection performance. However, in the relevant literature, the effectiveness of this method has only been proven on pure molybdenum and some molybdenum alloys with low alloying degree.

[0005] Thesis “Oxidation behavior of a MoSiBTiC alloy coated by a(Si+B)co-deposition pack

[0006] In the "cementation method", a Mo5Si3-MoSi2-SiO2 composite coating was prepared on a molybdenum-based composite material mixed with carbide particles by a method similar to the above-mentioned CN108118340A. However, during the embedding process, the carbides could not be completely converted into silicides and remained in the coating in large quantities, resulting in large residual stress, which caused the coating to crack and fail quickly during the subsequent high-temperature oxidation process. From this result, it can be seen that the oxidation-resistant coating (silicide coating) prepared by the existing embedding technology is extremely sensitive to the composition and organizational characteristics of the molybdenum-based alloy, and has a limited scope of application.

[0007] Therefore, it is of great practical significance to design and develop a new coating preparation method to solve the problem that the existing coating prepared by the embedding infiltration method cannot cope with a variety of alloy compositions and structures, further improve the application scope of the coating preparation method, reduce costs, shorten time, and realize the efficient and high-performance preparation of molybdenum-based alloy high-temperature protective coatings. Summary of the invention

[0008] Aiming at the problem that the anti-oxidation coating (silicide coating) prepared by the existing embedding infiltration technology is highly sensitive to the composition and organizational characteristics of molybdenum-based alloys, the present invention, based on the conventional embedding infiltration method, designs a coating preparation method with a wide range of applications, simple process and low cost, optimizes the parameters such as time, temperature, powder composition and the like used in the embedding infiltration process, and simultaneously performs a high-temperature short-time heat treatment on the coating after the embedding infiltration treatment, so as to obtain a coating with small residual stress, close bonding with the substrate and excellent high-temperature protection. This method is not only applicable to common pure molybdenum, TZM alloy and other molybdenum alloys, but also has good anti-oxidation performance for molybdenum-based composite materials with high alloying degree and inclusions of carbides and oxide particles, showing excellent applicability. In addition, compared with the traditional preparation technology of molybdenum-based alloy anti-oxidation coating, this process is simple to operate and has a short production process, which effectively reduces the cost required to prepare the coating.

[0009] The complete technical solution of the present invention includes:

[0010] A method for preparing a molybdenum-based alloy high-temperature protective coating comprises the following steps:

[0011] (1) Pretreatment of the coated substrate: Prepare a molybdenum-based alloy with a composition of (>50) Mo–(0-10) Si–(0-15) B–(0-15) Ti–(0-15) C (at.%) and cut it into small pieces. The edges and corners of the sample are rounded and passivated, and the surface is polished to 2000 mesh with sandpaper.

[0012] (2) Pretreatment of embedded infiltration mixed powder: Weigh Si, B and NaF powders, and grind the powders together using a planetary ball mill for more than 0.5 hours. Add Al2O3 powder to the ground powders, with a diameter of not less than 100 microns, and mix them evenly. The powder composition is (20-35)Si–(0-5)B–(2-5)NaF–Al2O3 (wt.%).

[0013] (3) Embedding infiltration treatment: Place the mixed powder obtained in step (2) into an alumina crucible, and then fill the sample in step (1) into the mixed powder, gently smooth the surface of the powder and cover the crucible with a lid. Place the crucible and the sample in a high-temperature furnace that can evacuate and adjust the atmosphere, and then evacuate the air. After the evacuation is completed, introduce argon gas. Set the sintering temperature to 900-1300℃, the heating rate to 10-30℃ / min, and the insulation time to 10-50 hours for embedding infiltration treatment. Cool the crucible and the sample to room temperature with the furnace and take them out. After removing the powder, a molybdenum-based alloy sample with a silicide coating is obtained.

[0014] (4) High-temperature short-time heat treatment: The sample with the silicide coating is subjected to high-temperature heat treatment. The furnace is first evacuated and then argon is introduced. The heat treatment adopts a step-by-step heating process. The heating rate from room temperature to 800°C is 20°C / min, and the heating rate from 800-1500°C is not higher than 5°C / min. After keeping at 1500°C for 0-5min, the temperature is stepped down. The cooling rate between 1500-600°C is not higher than 5°C / min. The sample is taken out after natural furnace cooling to room temperature below 600°C.

[0015] Furthermore, the molybdenum-based alloy high-temperature protective coating obtained by the above method is composed of MoSi2, Mo5Si3, Mo5SiB2 (T2) and MoB, and the coating includes Mo5SiB2+MoB layer, M5Si3 layer and MoSi2 layer in sequence from the substrate to the outside, and carbides (SiC and TiC) are distributed in each layer in a dispersed manner.

[0016] Furthermore, after the coating was cyclically oxidized at 1400°C for 100 hours, a glassy SiO2 oxide film was formed on the surface, and the thickness of the oxide film did not exceed 10 microns. The thickness of each layer below the coating increased slightly, but the overall structure did not change.

[0017] After the coating is oxidized at 1300℃ and 1400℃ for 100 hours, the weight increase of the sample does not exceed 2mg / cm 2 .

[0018] Furthermore, a molybdenum-based alloy with the above-mentioned high-temperature protective coating.

[0019] In the above scheme, the present invention designs the powder components of embedded infiltration. Compared with silicon infiltration alone, silicon-boron infiltration can form a continuous layer of Mo5SiB2(T2)+MoB on the inner side of the infiltration layer, which can inhibit the diffusion rate of silicon elements in the outer infiltration layer into the matrix, thereby extending the service life of the coating. The use of Al2O3 powder with a larger particle size (not less than 100μm) can retain larger gaps in the mixed powder, so that the reaction of Si, B and NaF in the gap is faster and more sufficient, and the diffusion efficiency of embedded infiltration is improved; at the same time, the large-particle Al2O3 powder can also prevent the sintering of the mixed powder during the embedded infiltration process, making the sample easier to demold.

[0020] At the same time, in the embedding infiltration process, if the embedding infiltration treatment temperature is too low, the coating will grow slowly and be inefficient; while if the temperature is too high, the silicon element on the surface of the formed coating will dissipate again, and the expected coating structure cannot be obtained, and the high-temperature oxidation resistance will not increase but will decrease. Within the above conditions, the present invention selects a suitable temperature and time according to the target thickness of the coating, and can efficiently prepare a protective coating.

[0021] In particular, the present invention adopts high-temperature short-time heat treatment after the embedding infiltration treatment. During the embedding infiltration process, the volume changes of the molybdenum alloy substrate with complex microstructure when each component of the substrate is transformed into silicide are different. Therefore, in addition to the thermal stress generated by the mismatch of thermal expansion coefficients at the common coating / substrate interface, a large amount of residual stress or micro cracks will also be generated at the grain boundaries inside the coating, which can easily cause the coating to crack and fail during the subsequent oxidation process. The present invention adds a high-temperature heat treatment process after the embedding infiltration treatment, which can relieve the internal stress in the coating and further promote the homogenization of the components in the coating; and the extremely short insulation time can also ensure that the Si and B elements in the coating have no time to escape, ensuring that the properties of the coating do not change. The slow heating and cooling rate around 1500°C is to avoid new thermal stress in the coating as much as possible, and the appropriate increase in the heating and cooling rate at the initial stage of heating and the later stage of cooling does not affect the effect of this heat treatment, and can also shorten the time and improve efficiency.

[0022] The present invention proposes a molybdenum-based alloy coating preparation technology with a wide range of applications, simple process and low cost. Compared with the prior art, the present invention has the following main features:

[0023] (1) Excellent coating performance: The coating prepared by this method still maintains good protective performance under the minimum cyclic oxidation conditions of 1400℃ / 200 hours. After the oxidation test, a dense and continuous SiO2 oxide film is formed on the surface. The microstructure of the coating does not change, and the thickness does not change significantly.

[0024] (2) Wide range of applications: High-temperature short-time heat treatment after embedding can relieve the residual internal stress in the coating without affecting the microstructure of the coating, avoiding cracking and failure caused by residual stress during subsequent oxidation, and greatly improving the high-temperature oxidation resistance of the coating. In addition to being suitable for pure molybdenum, TZM alloys and other common molybdenum-based alloys, the coating prepared by this method also has excellent performance for materials such as molybdenum-based composite materials reinforced with carbides and oxide particles that are prone to internal stress leading to coating cracking.

[0025] (3) Simple process and low cost: This coating preparation technology has simple requirements for equipment and raw materials, and has few restrictions on the composition, microstructure, and structural size of the molybdenum-based alloy matrix. It also performs well on large components with complex shapes. At the same time, this method shortens the coating preparation time and improves processing efficiency by adjusting the conditions of the embedding infiltration treatment, including increasing the treatment temperature and selecting a powder component ratio with a faster reaction rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The invention discloses a high temperature protective coating which is prepared on a molybdenum-based alloy by adopting the method of the invention.

[0027] Figure 2 This is the cross-sectional microstructure of the coating after cyclic oxidation at 1400°C for 100 hours.

[0028] Figure 3 Cyclic oxidation curves of the coating at 1300℃ and 1400℃. DETAILED DESCRIPTION

[0029] The present invention is described in detail below in conjunction with the embodiments and drawings, but it should be understood that the embodiments and drawings are only used to exemplify the present invention and do not constitute any limitation on the protection scope of the present invention. All reasonable changes and combinations within the scope of the inventive concept of the present invention fall within the protection scope of the present invention.

[0030] A method for preparing a molybdenum-based alloy high-temperature protective coating comprises the following steps:

[0031] (1) Pretreatment of the coated substrate: Prepare a molybdenum-based alloy with a composition of (>50) Mo–(0-10) Si–(0-15) B–(0-15) Ti–(0-15) C (at.%) and cut it into small pieces. The edges and corners of the sample are rounded and passivated, and the surface is polished to 2000 mesh with sandpaper.

[0032] (2) Pretreatment of embedded infiltration mixed powder: Weigh Si, B and NaF powders, and grind the powders together using a planetary ball mill for more than 0.5 hours. Add Al2O3 powder to the ground powders, with a diameter of not less than 100 microns, and mix them evenly. The powder composition is (20-35)Si–(0-5)B–(2-5)NaF–Al2O3 (wt.%).

[0033] (3) Embedding infiltration treatment: Place the mixed powder obtained in step (2) into an alumina crucible, and then fill the sample in step (1) into the mixed powder, gently smooth the surface of the powder and cover the crucible with a lid. Place the crucible and the sample in a high-temperature furnace that can evacuate and adjust the atmosphere, and then evacuate the air. After the evacuation is completed, introduce argon gas. Set the sintering temperature to 900-1300℃, the heating rate to 10-30℃ / min, and the insulation time to 10-50 hours for embedding infiltration treatment. Cool the crucible and the sample to room temperature with the furnace and take them out. After removing the powder, a molybdenum-based alloy sample with a silicide coating is obtained.

[0034] (4) High-temperature short-time heat treatment: The sample with the silicide coating is subjected to high-temperature heat treatment. The furnace is first evacuated and then argon is introduced. The heat treatment adopts a step-by-step heating process. The heating rate from room temperature to 800°C is 20°C / min, and the heating rate from 800-1500°C is not higher than 5°C / min. After keeping at 1500°C for 0-5min, the temperature is stepped down. The cooling rate between 1500-600°C is not higher than 5°C / min. The sample is taken out after natural furnace cooling to room temperature below 600°C.

[0035] The present invention proposes an efficient and reliable coating preparation method. By adjusting the existing embedded infiltration coating preparation method, the embedded infiltration treatment temperature is increased, the time is shortened, and the embedded infiltration powder composition is optimized according to the composition of the substrate; a high-temperature short-time heat treatment is performed on the embedded infiltration sample, and by setting a suitable heating rate, temperature and insulation time, the residual internal stress of the coating is released without affecting the coating structure, thereby realizing the preparation of a high-density, low residual stress high-temperature protective coating, and greatly improving the high-temperature oxidation resistance of the molybdenum-based alloy.

[0036] like Figure 1 As shown in the figure, the high temperature protective coating prepared on the molybdenum-based alloy by this method has a total thickness of 120 microns and contains MoSi2, Mo5Si3, Mo5SiB2 (T2), MoB and SiC. From the figure, it can be seen that from the substrate to the outside, it includes Mo5SiB2 + MoB layer, M5Si3 layer and MoSi2 layer in sequence. These three layers basically constitute a continuous layer, and SiC and TiC are dispersed in each layer. Figure 2 As shown in the figure, after the coating was cyclically oxidized at 1400℃ for 100 hours, a glassy SiO2 oxide film with a thickness of no more than 10 microns was formed on the surface, and the thickness of the layers below increased slightly, but the overall structure did not change. Figure 3 As shown in the figure, after the coating was oxidized at 1300℃ and 1400℃ for 100 hours, the sample not only did not lose weight, but also gained less than 2mg / cm 2 .

[0037] Example 1

[0038] (1) Pretreatment of the coated substrate: Prepare a molybdenum-based alloy with a composition of Mo–5Si–10B–10Ti–10C (at.%) and cut it into small pieces. The edges and corners of the sample are rounded and passivated, and the surface is polished to 2000 mesh with sandpaper.

[0039] (2) Pretreatment of embedded infiltration mixed powder: Weigh three kinds of powders, Si, B and NaF, and mix and grind the powders using a planetary ball mill for 0.5 hours. Add Al2O3 powder with a diameter of 150 microns to the ground powder and mix them evenly. The powder composition is 30Si–5B–2.5NaF–Al2O3 (wt.%).

[0040] (3) Embedding infiltration treatment: Place the mixed powder obtained in step (2) into an alumina crucible, and then fill the sample in step (1) into the mixed powder, gently smooth the surface of the powder and cover the crucible with a lid. Place the crucible and the sample in a high-temperature furnace that can evacuate and adjust the atmosphere, and then evacuate the air. After the evacuation is completed, introduce argon gas. Set the sintering temperature to 1200°C, the heating rate to 20°C / min, and the insulation time to 12 hours for embedding infiltration treatment. Cool the crucible and the sample to room temperature with the furnace and take them out. After removing the powder, a molybdenum-based alloy sample with a silicide coating is obtained.

[0041] (4) High-temperature short-time heat treatment: The sample with the silicide coating is subjected to high-temperature heat treatment. The furnace is first evacuated and then argon is introduced. The heat treatment adopts a step-by-step heating process. The heating rate from room temperature to 800°C is 20°C / min, and the heating rate from 800-1500°C is 5°C / min. After keeping at 1500°C for 1 minute, the temperature is stepped down. The cooling rate between 1500-600°C is 5°C / min. The sample is taken out after natural furnace cooling to room temperature below 600°C.

[0042] Example 2

[0043] (1) Pretreatment of the coated substrate: Prepare a molybdenum-based alloy with a composition of Mo-28Ti-14Si-6C-6B (at.%) and cut it into small pieces. The edges and corners of the sample are rounded and passivated, and the surface is polished to 2000 mesh with sandpaper.

[0044] (2) Pretreatment of embedded infiltration mixed powder: Weigh three kinds of powders, Si, B and NaF, and mix and grind the powders in a planetary ball mill for 1 hour. Add Al2O3 powder with a diameter of 200 microns to the ground powder and mix them evenly. The powder composition is 34Si–1B–2.5NaF–Al2O3 (wt.%).

[0045] (3) Embedding infiltration treatment: Place the mixed powder obtained in step (2) into an alumina crucible, and then fill the sample in step (1) into the mixed powder, gently smooth the surface of the powder and cover the crucible with a lid. Place the crucible and the sample in a high-temperature furnace that can evacuate and adjust the atmosphere, and then evacuate the air. After the evacuation is completed, introduce argon gas. Set the sintering temperature to 1000°C, the heating rate to 15°C / min, and the insulation time to 50 hours for embedding infiltration treatment. Cool the crucible and the sample to room temperature with the furnace and take them out. After removing the powder, a molybdenum-based alloy sample with a silicide coating is obtained.

[0046] (4) High-temperature short-time heat treatment: The sample with the silicide coating is subjected to high-temperature heat treatment. The furnace is first evacuated and then argon is introduced. The heat treatment adopts a step-by-step heating process. The heating rate from room temperature to 800°C is 20°C / min, and the heating rate from 800-1500°C is 5°C / min. After heating to 1500°C, the temperature is immediately lowered in steps. The cooling rate between 1500-600°C is 5°C / min. The sample is taken out after the temperature is naturally cooled to room temperature below 600°C.

[0047] The above applications are only some implementation methods of the present application. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A method for preparing a molybdenum-based alloy high-temperature protective coating, characterized in that: The steps include: (1) Pretreatment of the coated substrate: preparation of molybdenum-based alloy and passivation and surface treatment; (2) Pretreatment of embedded mixed powder: weigh Si, B and NaF powders, add Al2O3 powder and mix evenly. The diameter of Al2O3 powder should not be less than 100 μm. (3) embedding infiltration treatment: the mixed powder obtained in step (2) is placed in an alumina crucible, and the alloy obtained in step (1) is then embedded in the mixed powder. The crucible and the alloy are placed in a high-temperature furnace, evacuated, and then argon gas is introduced and embedding infiltration treatment is performed. The temperature is 900-1300°C, the heating rate is 10-30°C / min, and the holding time is 10-50 hours. After cooling to room temperature in the furnace, the mixture is taken out and the powder is removed to obtain a molybdenum-based alloy with a silicide coating. (4) High-temperature short-time heat treatment: The molybdenum-based alloy with silicide coating is subjected to high-temperature short-time heat treatment. The heat treatment adopts a step-temperature heating process, specifically: the heating rate from room temperature to 800°C is 20°C / min, and the heating rate from 800-1500°C is not higher than 5°C / min; after keeping at 1500°C for 0-5min, the temperature is stepped down, specifically: the cooling rate between 1500-600°C is not higher than 5°C / min, and the alloy is taken out after natural furnace cooling to room temperature below 600°C.

2. The method for preparing a molybdenum-based alloy high-temperature protective coating according to claim 1, characterized in that: In step (1), the molybdenum-based alloy composition is: Mo>45%, Si: 0-10%, B: 0-15%, Ti: 0-15%, C: 0-15%, and the above composition is atomic ratio.

3. The method for preparing a molybdenum-based alloy high-temperature protective coating according to claim 2, characterized in that: In step (1), the molybdenum-based alloy is cut into small pieces, the edges and corners of the alloy are subjected to rounding passivation treatment, and then the surface is polished to 2000 mesh.

4. The method for preparing a molybdenum-based alloy high-temperature protective coating according to claim 3, characterized in that: In step (2), the powder composition is: Si: 20%-35%, B: 0-5%, NaF: 2%-5%, and the rest is Al2O3, and the above composition is by weight ratio.

5. The method for preparing a molybdenum-based alloy high-temperature protective coating according to claim 4, characterized in that: In step (2), after weighing three kinds of powders of Si, B and NaF, the powders are mixed and ground using a planetary ball mill for more than 0.5 hours, and then Al2O3 powder is added to the ground powders.

6. The method for preparing a molybdenum-based alloy high-temperature protective coating according to claim 5, characterized in that: In step (4), before the alloy is subjected to high-temperature short-time heat treatment, the furnace is first evacuated and then argon gas is introduced, and then the heat treatment is started.

7. The molybdenum-based alloy high-temperature protective coating obtained by the method of claims 1-6 is characterized in that: The coating consists of MoSi2, Mo5Si3, Mo5SiB2(T2) and MoB.

8. The molybdenum-based alloy high-temperature protective coating according to claim 7, characterized in that: The coating includes a Mo5SiB2+MoB layer, a M5Si3 layer and a MoSi2 layer in sequence from the substrate to the outside, and carbides are dispersedly distributed in each layer.

9. The molybdenum-based alloy high-temperature protective coating according to claim 7, characterized in that: After the coating is cyclically oxidized at 1400° C. for 100 hours, a layer of glassy SiO2 oxide film is generated on the surface of the coating, and the thickness of the oxide film does not exceed 10 microns.

10. A molybdenum-based alloy having a coating according to any one of claims 7 to 9.

Citation Information

Cited By

  • Gas phase aluminizing method for nickel-based single crystal superalloy turbine blade

    CN122189558A