Photoelectric double-response light modulator and preparation method and application thereof

By combining WO3 electrochromic film and photochromic WO3 hydrogel electrolyte in electrochromic devices, a photoelectric dual-response dimmer is solved, and the problem of limited light transmittance loss and contrast adjustment in the prior art is achieved, and high efficiency is achieved Optical contrast adjustment and high light transmittance.

CN119002139AInactive Publication Date: 2024-11-22SHANDONG UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411121149.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing electrochromic devices have limited light transmittance loss and contrast adjustment in the bleached state, and the hydrogel electrolyte has a single effect, making it difficult to achieve efficient optical contrast adjustment.

Method used

The WO3 electrochromic film was prepared by pulse deposition method, and combined with the photochromic WO3 hydrogel electrolyte, a photoelectric dual-response dimmer was formed, which improved optical contrast and light transmittance through the synergistic effect of electrochromic and photochromic.

Benefits of technology

It realizes efficient optical contrast adjustment, reduces energy consumption, improves bleaching transmittance and contrast, and has a simple preparation process and excellent scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119002139A_ABST
    Figure CN119002139A_ABST
Patent Text Reader

Abstract

The invention discloses a photoelectric double-response light modulator and a preparation method and application thereof, and relates to the technical field of light modulators. The photoelectric double-response dimmer comprises a cathode, an anode and a hydrogel electrolyte, the hydrogel electrolyte is arranged between the cathode and the anode, and the hydrogel electrolyte is a photochromic WO3 hydrogel electrolyte; the cathode comprises a cathode substrate, and an electrochromic film is deposited on the cathode substrate. The electrochromic WO3 film is prepared by using a simple electrodeposition method, the photochromic WO3 hydrogel is prepared, the electrochromic WO3 film and the photochromic WO3 hydrogel are combined, the dimmer with a photoelectric double-response synergistic effect is prepared, the energy consumption is greatly reduced, and the optical contrast ratio is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of dimmer technology, specifically a photoelectric dual-response dimmer, its preparation method, and its application. Background Art

[0002] Electrochromic color modulators possess the ability to dynamically adjust transmittance, showing great application potential in green buildings, AR glasses, and other fields. However, achieving high transmittance contrast at the device level remains a challenging goal for electrochromic technology. Emerging zinc-anode-based electrochromic devices utilize dual electrochromic electrodes, significantly reducing colored transmittance. However, the presence of two electrochromic electrodes also introduces transmittance loss during the bleaching process.

[0003] Meanwhile, the transmittance loss of electrochromic devices in the bleached state is mainly attributed to the indium tin oxide (ITO) layer. Reducing the use of the ITO layer can maximize the bleached transmittance of the electrochromic device and significantly reduce the production cost. Zinc anode-based electrochromic devices can improve the bleached transmittance of the device by designing the framework structure of the zinc anode to eliminate the use of the counter electrode (e.g., ITO glass).

[0004] Besides the transmittance loss of the electrodes, the transmittance loss of the electrolyte also affects the transmittance contrast of the device. Among current electrolyte choices, hydrogel electrolytes are promising candidates for next-generation materials due to their excellent ionic conductivity and high transparency. However, the inventors have discovered that hydrogel electrolytes in existing electrochromic devices merely function as electrolytes themselves. The degree to which such electrochromic devices change optical contrast is only affected by photochromism, resulting in limited adjustment of optical contrast. Summary of the Invention

[0005] The purpose of this invention is to provide a photoelectric dual-response dimmer, its preparation method, and its application. An electrochromic WO3 thin film and a photochromic WO3 hydrogel are prepared using a simple electrodeposition method. By combining the electrochromic WO3 thin film and the photochromic WO3 hydrogel, a dimmer with photoelectric dual-response synergy is prepared, which greatly reduces energy consumption and improves optical contrast. The preparation method is simple, and the performance is superior to that of commercial electrochromic dimmers, thus solving the problems in the prior art.

[0006] To solve the above technical problems, the present invention is achieved through the following technical solutions:

[0007] The first aspect of the present invention provides a photoelectric dual-response dimmer.

[0008] A photoelectric dual-response dimmer includes a cathode, an anode, and a hydrogel electrolyte, wherein the hydrogel electrolyte is disposed between the cathode and the anode, and the hydrogel electrolyte is a photochromic WO3 hydrogel electrolyte; the cathode includes a cathode substrate, on which an electrochromic thin film is deposited.

[0009] As an optional technical solution, the electrochromic film is a WO3 electrochromic film; the anode includes an anode substrate on which a zinc frame or zinc foil is disposed; the cathode substrate is an ITO / PET conductive film and the anode substrate is a PET film; or, the cathode substrate is ITO conductive glass and the anode substrate is quartz glass.

[0010] Alternatively, a PET film can be used to encapsulate the cathode, anode, and hydrogel electrolyte;

[0011] Alternatively, the cathode, anode, and hydrogel electrolyte layers can be separated by 3M tape.

[0012] The second aspect of this invention provides a method for preparing a photoelectric dual-response dimmer.

[0013] A method for fabricating a photoelectric dual-response dimmer based on the first aspect includes the following steps:

[0014] Preparation of anode materials and cathode materials with deposited WO3 electrochromic thin films;

[0015] Preparation of photochromic WO3 hydrogel electrolyte;

[0016] A photochromic WO3 hydrogel electrolyte is placed between the anode and cathode materials and then encapsulated and fixed to obtain a photoelectric dual-response dimmer.

[0017] As an alternative technical solution, the preparation of the cathode material with deposited WO3 electrochromic thin film specifically includes:

[0018] The cathode substrate was ultrasonically cleaned and dried sequentially with deionized water, acetone, ethanol, and deionized water.

[0019] Na2WO4·2H2O was dissolved in deionized water, and HClO and H2O2 were added to prepare a precipitation solution containing WO3.

[0020] WO3 was deposited onto a cathode substrate using a pulse deposition method to obtain a cathode material with a WO3 electrochromic thin film deposited on it.

[0021] As an alternative technical solution:

[0022] In 100 ml of deionized water, the amount of Na2WO4·2H2O added is 0.2-0.45 g, and the amounts of HClO and H2O2 are 0.5-1 ml and 0.2-0.4 ml, respectively; preferably, the amounts of HClO and H2O2 are 0.8-1 ml and 0.2-0.3 ml, respectively.

[0023] In the pulse deposition method, the pulse voltage is set to -0.8 to -0.6V, 0.1 to 0.5s and 0 to 0.2V, 0.8 to 1.2s, and the number of pulse deposition cycles is 2000 to 5000.

[0024] As an optional technical solution, the preparation of the photochromic WO3 hydrogel electrolyte specifically includes:

[0025] Zinc perchlorate and lithium perchlorate or aluminum perchlorate are added to the pre-prepared WO3 particle colloid to obtain a conductive salt solution;

[0026] Acrylamide monomer, crosslinking agent, initiator and crosslinking agent auxiliaries are added to a conductive salt solution, mixed evenly, and then thermosetting to obtain photochromic WO3 hydrogel electrolyte.

[0027] As an optional technical solution, the method for preparing the WO3 particulate colloid specifically includes:

[0028] Hydrated tungsten oxide was prepared by anodic oxidation.

[0029] Hydrated tungsten oxide is added to water and dispersed evenly. Then ethylene glycol is added, the mixture is sealed, and heated to 95-98℃. The reaction is carried out for 20-30 minutes to obtain transparent WO3 granular colloid.

[0030] In the sealed reaction system, the volume ratio of water to ethylene glycol is 2–10:4–10.

[0031] As an alternative technical solution, anodic oxidation is used to prepare hydrated tungsten oxide, specifically as follows:

[0032] Place the tungsten sheet in hydrochloric acid electrolyte, apply a DC bias voltage of 40-60V to the tungsten sheet, treat for 20-30 minutes, seal and heat to 95-98℃, and react for 20-30 minutes.

[0033] The reaction product was washed with water and centrifuged to obtain a precipitate, thus preparing hydrated tungsten oxide.

[0034] As an alternative technical solution:

[0035] In the conductive salt solution, the concentration of zinc perchlorate is 0.2–1 mol / L, preferably 0.1–0.2 mol / L; the concentration of lithium perchlorate or aluminum perchlorate is 0.8–2 mol / L, preferably 0.8–1 mol / L.

[0036] The mass ratio of acrylamide monomer to the volume of conductive salt solution is 0.2–0.5 g:1 mL, preferably 0.3–0.4 g:1 mL;

[0037] The mass of the crosslinking agent is 0.5-1% of the mass of the acrylamide monomer, and the mass of the crosslinking agent auxiliaries is 0.1-0.2% of the mass of the acrylamide monomer;

[0038] The crosslinking agent is N,N'-methylenebisacrylamide; the crosslinking agent auxiliary is N,N,N',N'-tetramethylethylenediamine; and the initiator is ammonium persulfate.

[0039] The heat curing temperature is 30–50℃, and the heat curing time is 15–20 min.

[0040] A third aspect of the present invention provides an application of a photoelectric dual-response dimmer in AR glasses.

[0041] The present invention has the following beneficial effects:

[0042] 1. This invention discloses a photoelectric dual-response dimmer, its preparation method, and its application. Addressing the technical problem that the degree of change in optical contrast of existing electrochromic devices is only affected by photochromism alone, resulting in a limited degree of adjustment of optical contrast, this invention proposes and prepares a dimmer with photoelectric dual-response synergy, which can superimpose the dual dimming effects of photochromism and electrochromism, thereby improving the degree of adjustment of optical contrast and greatly reducing energy consumption.

[0043] 2. The WO3 electrochromic film prepared by this invention has a simple preparation process, and the WO3 film achieves high bleaching transmittance, greater than 90% in the visible light range. The response time of the WO3 electrochromic film is the fading time t. b = 1.7s, coloring time t c =4.9s, while achieving an optical contrast ratio of 52.1%. The use of pulse deposition technology also facilitates morphology control and provides excellent scalability.

[0044] 3. The photochromic WO3 gel electrolyte proposed in this invention has high transmittance (~90%) and high optical contrast (~90%). It also exhibits rapid light response. The minimum color transmittance is below 5% in the visible light band, and the gel electrolyte also possesses high ionic conductivity, enabling it to be used as an electrolyte in dimmers to enhance dimmer functionality.

[0045] 4. The photoelectric dual-response dimmer prepared by this invention has a high transmittance contrast (83.1% at 633 nm) and maintains high transparency (85.3%) in the bleached state. This dimmer incorporates photochromic WO3 gel as the electrolyte, and due to the electrolyte's corrosion resistance, the dimmer exhibits significantly enhanced cycling stability (87.2% of the initial optical contrast is retained after 1000 cycles). The dimmer possesses advantages such as simple synthesis process, high reversible color-changing efficiency, and long cycle life.

[0046] 5. The photoelectric dual-response Zn-WO3 dimmer of this invention can be used not only for sunlight and solar thermal management, but also for flexible lenses in wearable AR glasses. The flexible Zn-WO3 dimmer can provide more intermediate color states and a near-opaque state, which improves the visual performance of AR glasses, surpassing commercially available XREALAir 2Pro AR glasses equipped with electrochromic lenses. The raw materials used are inexpensive and readily available, and are non-toxic and harmless to the environment. Furthermore, given its excellent performance in terms of rapid response and reversibility, coupled with a simple manufacturing and operating process, the Zn-WO3 dimmer shows broad promise in areas such as smart windows, augmented reality, virtual reality, and transparent displays.

[0047] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description

[0048] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0049] Figure 1(a) is the XRD pattern of the WO3 electrochromic thin film prepared in Example 1.

[0050] Figure 1(b) is a cross-sectional SEM image of the WO3 electrochromic film.

[0051] Figure 2(a) shows the transmittance curves of the WO3 electrochromic film prepared in Example 1 at different voltages (the inset shows the actual images at the corresponding voltages).

[0052] Figure 2(b) shows the transmittance of the WO3 electrochromic film during the coloring / fading process at a wavelength of 633 nm as a function of time.

[0053] Figure 3(a) shows the WO3 electrochromic film prepared in Example 1 after 1000 CV cycles in a PC-based electrolyte.

[0054] Figure 3(b) shows the transmittance change spectrum of the WO3 electrochromic film at a wavelength of 633 nm during 1000 switching cycles in a PC-based electrolyte.

[0055] Figure 4(a) is a schematic diagram of the rigid photoelectric dual-response Zn-WO3 dimmer prepared in Example 1.

[0056] Figure 4(b) shows the physical display of the rigid photoelectric dual-response Zn-WO3 dimmer under different illumination times and the synergistic effect of photoelectric color change.

[0057] Figure 5 The image shows a physical display of the rigid photoelectric dual-response Zn-WO3 dimmer prepared in Example 2 applied to eyeglass lenses.

[0058] Figure 6(a) is a schematic diagram of the structure of the flexible optoelectronic dual-response Zn-WO3 dimmer prepared in Example 3.

[0059] Figure 6(b) shows the physical display of the flexible optoelectronic dual-response Zn-WO3 dimmer in different states.

[0060] Figure 6(c) shows the transmittance curves of the flexible optoelectronic dual-response Zn-WO3 dimmer under different conditions.

[0061] Figure 7 The image shows the transmittance change spectrum of the WO3 electrochromic thin film prepared in Comparative Example 2 at a wavelength of 633 nm in an aqueous electrolyte during 300 switching cycles.

[0062] Figure 8(a) is a schematic diagram of the flexible optoelectronic dual-response Zn-WO3 dimmer prepared in Application Example 1 applied to commercial AR glasses.

[0063] Figure 8(b) shows the imaging display of the XREAL Air 2Pro AR glasses in three modes.

[0064] Figure 8(c) shows the imaging display of the flexible optoelectronic dual-response Zn-WO3 dimmer applied to four modes of commercial AR glasses. DETAILED DESCRIPTION

[0065] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention.

[0066] In a first aspect, the present invention provides a specific structure for a photoelectric dual-response dimmer.

[0067] A photoelectric dual-response dimmer includes a cathode, an anode, and a hydrogel electrolyte, wherein the hydrogel electrolyte is disposed between the cathode and the anode, and the hydrogel electrolyte is a photochromic WO3 hydrogel electrolyte; the cathode includes a cathode substrate, on which an electrochromic film is deposited; the electrochromic film is a WO3 electrochromic film.

[0068] As shown in Figures 4(a) and 6(a), it can be understood that the anode includes an anode substrate on which a zinc frame or zinc foil is disposed;

[0069] The cathode substrate is an ITO / PET conductive film, and the anode substrate is a PET film; or, the cathode substrate is ITO conductive glass, and the anode substrate is quartz glass; thus, a flexible photoelectric dual-response dimmer or a rigid photoelectric dual-response dimmer can be obtained.

[0070] It is understood that the photoelectric dual-response dimmer also uses a PET film to encapsulate the cathode, anode, and hydrogel electrolyte, thus achieving a monolithic structure. Furthermore, to prevent short circuits, each layer of the cathode, anode, and hydrogel electrolyte is separated by 3M tape.

[0071] Secondly, this invention provides a photoelectric dual-response dimmer, its preparation method, and its application, comprising the following steps:

[0072] (1) Preparation of WO3 electrochromic thin film

[0073] The steps include:

[0074] The ITO glass, quartz glass, PET film, and ITO / PET conductive film were sequentially ultrasonically washed with deionized water, acetone, ethanol, and deionized water for 15 minutes, and then dried with nitrogen gas for later use.

[0075] Dissolve Na₂WO₄·2H₂O in 100 ml of deionized water and add HClO and H₂O₂ to prepare the precipitation solution. The amount of Na₂WO₄·2H₂O added to the deionized water is 0.2-0.45 g, and the amounts of HClO and H₂O₂ are 0.5-1 ml and 0.2-0.4 ml, respectively.

[0076] WO3 was deposited onto washed ITO glass or ITO / PET conductive film using a pulse deposition method to obtain an electrochromic WO3 film. The pulse voltage was set to -0.8 to -0.6V for 0.1–0.5 s and 0–0.2V for 0.8–1.2 s. The deposition cycle was 2000–5000.

[0077] In some embodiments, the amount of Na2WO4·2H2O is 0.4-0.45 grams.

[0078] Preferably, the amounts of HClO and H2O2 used are 0.8-1 ml and 0.2-0.3 ml, respectively.

[0079] In some embodiments, the pulse voltage is set to -0.7 to -0.6V, 0.1-0.2s and 0-0.1V, 0.8-1s.

[0080] In some embodiments, the number of pulse deposition cycles is 2000-4000.

[0081] In some embodiments, the electrochromic properties of the WO3 electrochromic film are measured in an oily electrolyte, and more preferably a propylene carbonate (PC)-based electrolyte. Studies have shown that free water molecules in aqueous electrolytes can cause the WO3 electrochromic film to dissolve, resulting in a significant decrease in its stability. Both PC-based electrolytes and hydrogel electrolytes contain a very small number of free water molecules, which can improve the cycling stability of the electrochromic film.

[0082] (2) Preparation of photochromic WO3 hydrogel electrolyte.

[0083] The steps include:

[0084] Hydrated tungsten oxide was prepared by anodizing. The anodizing process was as follows: a tungsten sheet was placed in a hydrochloric acid electrolyte, a DC bias voltage of 40-50V was applied to the tungsten sheet, and the treatment was carried out for 20-30 minutes.

[0085] After anodic oxidation, the precipitate, hydrated tungsten oxide, is obtained by washing with water and centrifugation. The centrifugation speed is 8000–12000 r / min, the time is 5–15 min, and the number of washes is 2–3.

[0086] Hydrated tungsten oxide was dispersed in water, and ethylene glycol was added. The mixture was then sealed, heated, and stirred. The volume ratio of ethylene glycol to water was 2–10:4–10. The heating temperature was 95–98°C. The reaction time was 20–30 minutes.

[0087] Using the reacted colloid as a solvent, zinc perchlorate and lithium perchlorate or aluminum perchlorate are added to the solvent to obtain a conductive salt solution. Acrylamide monomer, crosslinking agent, initiator and crosslinking agent auxiliaries are added to the conductive salt solution. After mixing evenly, the mixture is thermo-cured to obtain the hydrogel electrolyte.

[0088] In some embodiments, the crosslinking agent is N,N'-methylenebisacrylamide.

[0089] In some embodiments, the crosslinking agent is N,N,N',N'-tetramethylethylenediamine (TEMED).

[0090] In some embodiments, the heat curing temperature is 30–50°C and the heat curing time is 15–20 min.

[0091] In some embodiments, the initiator is ammonium persulfate. Ammonium persulfate is more uniformly dispersed in the reaction system, which is beneficial to the uniformity of crosslinking and curing, and avoids the generation of internal stress caused by uneven dispersion.

[0092] Specifically, a conductive salt solution is obtained by adding 0.1-1 mol / L zinc perchlorate and 0.8-2 mol / L lithium perchlorate to a solvent. 1.6 g of acrylamide monomer, N,N'-methylenebisacrylamide (MBAA, 13 mg), and ammonium persulfate (26 mg) as an initiator are then added to the conductive salt solution. After complete dissolution, a transparent colloid is obtained. Subsequently, 3 μL of N,N,N',N'-tetramethylethylenediamine (TEMED) is added to the above solution. After mixing thoroughly, the mixture is heat-cured at 60°C for 20 minutes to obtain the photochromic WO3 hydrogel electrolyte.

[0093] In some embodiments, the concentration of zinc perchlorate in the conductive salt solution is 0.2–1 mol / L, or 0.2–0.3 mol / L. Preferably, it is 0.1–0.2 mol / L.

[0094] In some embodiments, the concentration of lithium perchlorate or aluminum perchlorate in the conductive salt solution is 0.8–2 mol / L, or 0.9–1.1 mol / L. Preferably, it is 0.8–1 mol / L.

[0095] In some embodiments, the mass ratio of acrylamide monomer to the volume of conductive salt solution is 0.2–0.5 g:1 mL, more preferably 0.3–0.4 g:1 mL.

[0096] In some embodiments, the mass of the crosslinking agent is 0.5 to 1% of the mass of the acrylamide monomer, and the mass of the crosslinking agent auxiliaries is 0.1 to 0.2% of the mass of the acrylamide monomer. Studies have shown that under these conditions, the surface of the prepared gel electrolyte can remain smooth. When excessive amounts of crosslinking agent auxiliaries are added, the internal stress generated due to different solidification rates can cause wrinkling of the gel surface and affect the permeability of the final film.

[0097] (3) Fabrication and assembly of photoelectric dual-response Zn-WO3 dimmer

[0098] The above-mentioned WO3 electrochromic thin film and photochromic WO3 hydrogel electrolyte are used as photoelectric responsive active materials.

[0099] Rigid and flexible dual-response dimmers can be fabricated by varying the pulse deposition substrate. When the cathode substrate is an ITO / PET conductive film and the anode substrate is a PET film, a flexible optoelectronic dual-response dimmer can be fabricated, such as... Figure 6a As shown; when the cathode substrate is ITO conductive glass and the anode substrate is quartz glass, a rigid photoelectric dual-response dimmer can be fabricated, such as... Figure 4a As shown.

[0100] During the fabrication process, rigid dual-response dimmers and flexible dual-response dimmers can be freely selected according to actual needs, and this embodiment does not impose any restrictions on this.

[0101] When fabricating a rigid dual-response dimmer:

[0102] The electrochromic WO3 film and photochromic WO3 hydrogel electrolyte prepared in steps (1) and (2) are then processed according to... Figure 6a The structure shown was used to fabricate a 5*5cm photoelectric dual-response Zn-WO3 dimmer: a suitably sized WO3 hydrogel electrolyte and a zinc foil frame were placed between two side-by-side ITO / PET conductive films and a PET film. The ITO / PET conductive films were coated with a WO3 electrochromic layer. Each component was separated by 3M tape to prevent short circuits.

[0103] In some embodiments, the dimmer frame is manufactured using 3D printing technology and made of polytetrafluoroethylene (PTFE).

[0104] In some embodiments, the dimmer lens includes a flexible ITO / PET conductive film and a PET film arranged side by side. The ITO / PET conductive film is coated with a WO3 electrochromic layer, and a photochromic layer is disposed between the two films. The photochromic layer is made of the hydrogel electrolyte obtained in step (2) above.

[0105] In some embodiments, a zinc foil ring is laid around the edge of the hydrogel electrolyte as an electrochromic anode, and the zinc foil portion can be embedded in a groove designed into the frame to maintain aesthetics.

[0106] In some embodiments, the dimmer wires are led out through grooves in the temple, thereby concealing the wires within the temple.

[0107] Thirdly, the present invention provides the application of the dimmer in AR glasses.

[0108] When the dimmer is used in AR glasses, it can provide more adjustment levels and lower tint transmittance than commercial AR glasses.

[0109] This invention provides a pulsed electrodeposition method for preparing flexible tungsten oxide electrochromic films; hydrating tungsten oxide is prepared via anodic oxidation, and ultra-small tungsten oxide colloids are prepared via a solution method. These tungsten oxide colloids are then used to prepare a tungsten oxide photochromic hydrogel electrolyte with photochromic properties and high ionic conductivity. A Zn-WO3 dimmer with photoelectric dual response capability can be fabricated through rational device structure design. The Zn-WO3 dimmer prepared by this invention can achieve four dimming levels, ensuring excellent visual performance of AR glasses. Furthermore, compared to the outdoor mode of the XREAL Air 2Pro AR glasses, the Zn-WO3 dimmer provides a darker background. Moreover, the preparation method of this invention is simple, low-cost, and environmentally friendly.

[0110] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments and comparative examples.

[0111] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.

[0112] Example 1

[0113] A method for fabricating a photoelectric dual-response dimmer includes the following steps:

[0114] (1) Preparation of WO3 electrochromic thin film

[0115] ITO glass and quartz glass (10*40mm) 2 The sample was ultrasonically washed with deionized water, acetone, ethanol and deionized water for 15 minutes in sequence, and dried with nitrogen gas for later use. 0.412g of Na2WO4·2H2O was dissolved in 100ml of deionized water and 0.8ml of HClO and 0.26ml of H2O2 were added to prepare the sedimentation solution.

[0116] WO3 was deposited onto washed ITO glass by applying pulse voltages of -0.7V for 0.2s and 0V for 1s for 2000 cycles to obtain an electrochromic WO3 film.

[0117] (2) Preparation of PC-based electrolytes

[0118] 0.1M zinc perchlorate and 0.9M lithium perchlorate were dissolved in PC to form a PC-based electrolyte.

[0119] The electrochromic properties of the obtained WO3 electrochromic film were characterized: the WO3 electrochromic film was used as the working electrode, and zinc foil was used as the counter electrode and reference electrode, and the film was placed in the electrolyte prepared in step (2). An electrochemical workstation was connected to the two-electrode system for electrochemical performance characterization. Simultaneously, the electrochemical workstation was coupled with a UV-Vis spectrometer for electrochromic performance characterization. The structure of the electrodeposited WO3 film of this invention was determined by X-ray diffraction, as shown in the figure. Figure 1a As shown in the XRD pattern, the obtained material composition is amorphous WO3. The film thickness was observed using transmission electron microscopy. Figure 1b As shown, the thickness of the WO3 electrochromic film is approximately 377 nm. Figure 2a As shown, when a voltage of 0.1V is applied using an electrochemical workstation, the WO3 film exhibits a blue colored state; when a voltage of 1.5V is applied, the film is in a colorless bleached state. At a wavelength of 633nm, the transmittance modulation range of the WO3 film prepared in this embodiment is 52.1%, and the maximum transmittance is 93.7%. The color switching time t during the bleaching and coloring processes is also shown. b and t c These are defined as the time required to achieve 90% of the final modulation, respectively 1.7s and 4.9s. Figure 2b ).

[0120] The cycle life of the WO3 film was determined by cyclic voltammetry, and the film retained 77.67% of its initial capacity. Figure 3a It also retains 87.9% of its initial optical contrast after 1000 in-situ transmittance switching cycles. Figure 3b It exhibits excellent reversibility and repeatability.

[0121] (3) Preparation of photochromic WO3 hydrogel electrolyte

[0122] Place the tungsten sheet in hydrochloric acid electrolyte and apply a DC bias voltage of 40V to the tungsten sheet for 20 minutes.

[0123] After anodic oxidation, the precipitate, hydrated tungsten oxide, was obtained by washing with water and centrifugation. The centrifugation was performed at 8000 rpm for 10 minutes, with two washes. The hydrated tungsten oxide was then dispersed in water, and ethylene glycol was added. The mixture was then sealed, heated, and stirred. The volume ratio of ethylene glycol to water was 2:1, and the temperature was raised to 95°C. The reaction time was 30 minutes.

[0124] Using the reacted colloid as a solvent, 0.1 mol / L zinc perchlorate and 0.9 mol / L lithium perchlorate were added to the solvent to obtain a conductive salt solution. 1.6 g of acrylamide monomer, N,N'-methylenebisacrylamide (MBAA, 13 mg) and initiator ammonium persulfate (26 mg) were added to the conductive salt solution. After complete dissolution, a transparent colloid was obtained. Subsequently, 3 μL of N,N,N',N'-tetramethylethylenediamine (TEMED) was added to the above solution. After mixing evenly, the mixture was heat-cured at 60 °C for 20 minutes to obtain the photochromic WO3 hydrogel electrolyte.

[0125] (4) Fabrication of photoelectric dual-response Zn-WO3 dimmer

[0126] The electrochromic WO3 film and the photochromic WO3 hydrogel electrolyte prepared in steps (1) and (3) are then processed according to... Figure 4a The structure shown illustrates the fabrication of a 5*5cm rigid photoelectric dual-response Zn-WO3 dimmer: a suitably sized WO3 hydrogel electrolyte and a zinc sheet frame are placed between two side-by-side ITO conductive glass and quartz glass layers. The ITO conductive glass is coated with a WO3 electrochromic layer. Each layer is separated by 3M tape to prevent short circuits.

[0127] The photoelectric dual-response Zn-WO3 dimmer prepared in step (4) was placed under a uniform xenon lamp light source system with an illumination distance of 15 cm, a current of 15 A, and a voltage of 15 V to simulate the intensity of sunlight. Simultaneously, the light source system was coupled with an electrochemical workstation to characterize the photoelectric dual-response color change.

[0128] like Figure 4b As shown, the transparent dimmer has high transmittance, allowing the cartoon pattern behind the device to be clearly seen. With prolonged illumination, photochromism gradually takes effect, and the dimmer's color deepens. When voltage is applied to the dimmer, causing both photochromism and electrochromism to function simultaneously, the dimmer's transmittance drops to its minimum, and the cartoon pattern behind the device becomes almost invisible.

[0129] Example 2

[0130] A method for fabricating a photoelectric dual-response dimmer and its application, comprising the following steps:

[0131] (1) The preparation of the WO3 electrochromic thin film was the same as in Example 1.

[0132] (2) The preparation of the photochromic WO3 hydrogel electrolyte was the same as in Example 1.

[0133] (3) Fabrication of photoelectric dual-response Zn-WO3 dimmer

[0134] The photoelectric dual-response Zn-WO3 dimmer measures 2*4cm, and the zinc sheet frame is replaced with a more flexible zinc foil. The remaining steps are the same as in Example 1.

[0135] (4) Application of photoelectric dual-response Zn-WO3 dimmer

[0136] like Figure 5 As shown, a Zn-WO3 dimmer was embedded in a pair of eyeglasses and secured with glue. A laser pointer was used to generate a light spot, simulating a projection effect on the dimmer. As the illumination time increased, the dimmer's color deepened, and the light spot gradually became clearer. The clearest light spot image was produced when photochromism and electrochromism worked in tandem, and the image behind the glasses became invisible. This demonstrates the potential of the Zn-WO3 dimmer to enable switching between AR and VR.

[0137] Example 3

[0138] A method for fabricating a photoelectric dual-response dimmer and its application, comprising the following steps:

[0139] (1) Preparation of WO3 electrochromic thin film

[0140] The conductive substrate is a flexible ITO / PET conductive film. The ITO / PET conductive film and the PET film are cleaned separately. The WO3 electrochromic film is deposited on the ITO / PET conductive film. The remaining steps are the same as in Example 1.

[0141] (2) The preparation of the photochromic WO3 hydrogel electrolyte was the same as in Example 1.

[0142] (3) Fabrication of photoelectric dual-response Zn-WO3 dimmer

[0143] The electrochromic WO3 film and photochromic WO3 hydrogel electrolyte prepared in steps (1) and (2) are then processed according to... Figure 3a The structure shown illustrates the fabrication of a 5*5cm photoelectric dual-response Zn-WO3 dimmer: A suitably sized WO3 hydrogel electrolyte and a flexible zinc foil are placed between two side-by-side ITO / PET conductive films and a PET film. The ITO / PET conductive films are coated with a WO3 electrochromic layer. Each component is separated by 3M tape to prevent short circuits.

[0144] (4) Application of photoelectric dual-response Zn-WO3 dimmer

[0145] like Figure 6aAs shown, the frame was customized using 3D printing based on the dimensions of the Zn-WO3 dimmer, with grooves in the rim and temples to embed zinc foil and wires. The dimmer exhibits multiple levels of tinting in bleached (BS), photochromic (PC), electrochromic (EC) states, and a combination of photochromic and electrochromic states (PC+EC). Figure 6b The transmittance spectrum under the corresponding conditions is as follows: Figure 6c As shown, in the transparent state, the dimmer's transmittance can still reach about 70% at 633nm, and the transmittance in the colored state at 633nm can drop to as low as about 4.7%, which is close to the opaque state.

[0146] Comparative Example 1

[0147] The difference from Example 1 is that lithium perchlorate in step (3) is replaced with aluminum perchlorate, while the other steps remain unchanged. 3+ The presence of [a substance] causes hydrolysis of free water in the hydrogel before polymerization, reducing the number of free water molecules linking ethylene glycol and PAAm chains during polymerization, thus slowing down the hydrogel polymerization process. It also leads to a decrease in the photochromic effect of the corresponding hydrogel.

[0148] Comparative Example 2

[0149] The difference from Example 1 is that the electrolyte solvent in step (2) is replaced with water.

[0150] like Figure 7 As shown, the WO3 electrochromic film prepared in this comparative example exhibits poor cycling stability in an aqueous electrolyte. After 100 color-changing cycles, the electrochromic performance of the WO3 film significantly degrades, and after 300 color-changing cycles, the WO3 material completely loses its electrochromic properties and dissolves in the water. Therefore, using a gel electrolyte containing very few free water molecules can ensure the cycling stability of the WO3 electrochromic film.

[0151] Application Example 1

[0152] Application demonstration of photoelectric dual-response Zn-WO3 dimmer in commercial AR glasses

[0153] The preparation steps are as follows:

[0154] (1) Component assembly

[0155] Cleaning: Take ITO / PET conductive film and PET film (5×5cm) 2 The sample was ultrasonically washed with deionized water, acetone, ethanol and deionized water in sequence for 15 minutes, and then dried with nitrogen for later use.

[0156] Electrodeposition: As described in step (1) of Example 3, a WO3 electrochromic film was electrodeposited on the ITO / PET conductive film;

[0157] Prepare photochromic WO3 hydrogel electrolyte: as described in step (3) of Example 1, and cut the polymerized hydrogel electrolyte into appropriate sizes.

[0158] Assembly: Apply 0.5cm wide conductive copper tape around the edges of both prepared ITO / PET conductive films and PET films, pressing them firmly. Then, apply a layer of 3M transparent double-sided tape over the copper tape, ensuring the tape completely covers it without contacting the electrolyte. Next, attach the cut electrolyte to the surface of the ITO / PET conductive film, ensuring it adheres tightly to the WO3 film. Cut a zinc foil frame, ensuring that when attached to the double-sided tape on the glass, the edges protrude 3-5mm inwards and contact the electrolyte, without obstructing the WO3 film. Finally, cover with another PET film and press the two films together to assemble the electrochromic device.

[0159] Compaction: Place the device under a heavy object and compact it for 1-2 days;

[0160] (2) Imaging demonstration of Zn-WO3 dimmer on commercial AR glasses

[0161] like Figure 8a As shown, the prepared Zn-WO3 dimmer was installed on purchased commercial AR glasses (XREAL Air2Pro). The AR glasses can display three electrochromic dimming levels (home, travel, and outdoor modes). Figure 8b Zn-WO3 dimmers achieve four dimming levels by superimposing electrochromic and photochromic effects. Figure 8c These four dimming levels enhance adaptability to various lighting conditions, ensuring excellent visual performance for the AR glasses. Furthermore, compared to the outdoor mode of the XREAL Air 2 Pro AR glasses, the EC+PC state of the Zn-WO3 dimmer provides a significantly darker background, facilitating a seamless transition from AR to opaque VR glasses. These performance attributes highlight the potential of the flexible Zn-WO3 dimmer for AR glasses.

[0162] Throughout this specification, references to terms such as "one embodiment," "example," or "specific example" indicate that the specific features, structures, materials, or characteristics described in conjunction with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, schematic representations of these terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0163] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A photoelectric dual response dimmer, characterized in that: The invention comprises a cathode, an anode and a hydrogel electrolyte, wherein the hydrogel electrolyte is arranged between the cathode and the anode, and the hydrogel electrolyte is a photochromic WO3 hydrogel electrolyte; the cathode comprises a cathode substrate, and an electrochromic film is deposited on the cathode substrate.

2. The photoelectric dual response dimmer according to claim 1, characterized in that: The electrochromic film is a WO3 electrochromic film; the anode includes an anode substrate, on which a zinc frame or zinc foil is arranged; the cathode substrate is an ITO / PET conductive film, and the anode substrate is a PET film; or, the cathode substrate is an ITO conductive glass, and the anode substrate is a quartz glass; Alternatively, a PET film is provided to encapsulate the cathode, the anode and the hydrogel electrolyte; Alternatively, the cathode, anode and hydrogel electrolyte layers were separated by 3M tape.

3. A method for preparing the photoelectric dual-response dimmer according to any one of claims 1 to 2, characterized in that: The following steps are involved: Prepare anode material and cathode material with WO3 electrochromic film deposited thereon; Preparation of photochromic WO3 hydrogel electrolyte; The photochromic WO3 hydrogel electrolyte is placed between the anode material and the cathode material, and a photoelectric dual-response dimmer is obtained after encapsulation and fixation.

4. The method for preparing the photoelectric dual-response dimmer according to claim 3, characterized in that: The preparation of the cathode material deposited with a WO3 electrochromic thin film specifically comprises: The cathode substrate was ultrasonically washed with deionized water, acetone, ethanol and deionized water in sequence and then blown dry; Na2WO4·2H2O was dissolved in deionized water, and HClO and H2O2 were added to prepare a deposition solution containing WO3; WO3 is deposited on a cathode substrate by a pulse deposition method to obtain a cathode material on which a WO3 electrochromic thin film is deposited.

5. The method for preparing the photoelectric dual-response dimmer according to claim 4, characterized in that: In 100 ml of deionized water, the amount of Na2WO4·2H2O added is 0.2-0.45 g, the amounts of HClO and H2O2 used are 0.5-1 ml and 0.2-0.4 ml respectively; preferably, the amounts of HClO and H2O2 used are 0.8-1 ml and 0.2-0.3 ml respectively; In the pulse deposition method, the pulse voltage is set to -0.8-0.6V, 0.1-0.5s and 0-0.2V, 0.8-1.2s, and the number of pulse depositions is 2000-5000 cycles.

6. The method for preparing the photoelectric dual-response dimmer according to claim 3, characterized in that: The preparation of the photochromic WO3 hydrogel electrolyte specifically comprises: Adding zinc perchlorate and lithium perchlorate or aluminum perchlorate to the pre-prepared WO3 particle colloid to obtain a conductive salt solution; Add acrylamide monomer, crosslinking agent, initiator and crosslinking agent auxiliary into the conductive salt solution, mix them evenly, and then perform thermal curing to obtain the photochromic WO3 hydrogel electrolyte.

7. The method for preparing the photoelectric dual-response dimmer according to claim 6, characterized in that: The preparation method of the WO3 particle colloid specifically comprises: The hydrated tungsten oxide was prepared by anodization method; Add hydrated tungsten oxide to water and disperse evenly, then add ethylene glycol, seal and heat to 95-98℃, react for 20-30 minutes to obtain transparent WO3 particle colloid; Wherein, in the sealed reaction system, the volume ratio of water to ethylene glycol is 2-10:4-10.

8. The method for preparing the photoelectric dual-response dimmer according to claim 7, characterized in that: The hydrated tungsten oxide is prepared by anodizing, specifically: Place the tungsten sheet in a hydrochloric acid electrolyte, apply a DC bias voltage of 40 to 60 V to the tungsten sheet, treat for 20 to 30 minutes, seal and heat to 95 to 98°C, and the reaction time is 20 to 30 minutes; The reaction product is washed with water and centrifuged to obtain a precipitate to prepare hydrated tungsten oxide.

9. The method for preparing the photoelectric dual-response dimmer according to claim 6, characterized in that: In the conductive salt solution, the concentration of zinc perchlorate is 0.2 to 1 mol / L, preferably 0.1 to 0.2 mol / L; the concentration of lithium perchlorate or aluminum perchlorate is 0.8 to 2 mol / L, preferably 0.8 to 1 mol / L; The ratio of the mass of the acrylamide monomer to the volume of the conductive salt solution is 0.2-0.5 g:1 mL, preferably 0.3-0.4 g:1 mL; The mass of the cross-linking agent is 0.5-1% of the mass of the acrylamide monomer, and the mass of the cross-linking agent auxiliary is 0.1-0.2% of the mass of the acrylamide monomer; The crosslinking agent is N,N'-methylenebisacrylamide; the crosslinking agent auxiliary is N,N,N',N'-tetramethylethylenediamine; the initiator is ammonium persulfate; The temperature of thermal curing is 30-50°C, and the thermal curing time is 15-20 minutes.

10. Application of the optoelectronic dual-response dimmer according to any one of claims 1 to 2 in AR glasses.

Citation Information

Patent Citations

  • Prussian blue / tungsten trioxide electrochromic film and preparation method thereof

    CN109437241A

  • Composite hydrogel, preparation method, thermoelectric dual-drive composite hydrogel intelligent window and preparation method

    CN113896908A

  • Thermoelectric double-response intelligent color-changing device and preparation method thereof

    CN114137773A

  • Porous tungsten oxide film capable of independently regulating visible light and near-infrared light and preparation method of porous tungsten oxide film

    CN115259685A

  • High-stability hydrogel electrolyte for electrochromic device

    CN115963666A