Pole piece with multiple layers of solid electrolyte, preparation method of pole piece, solid-state battery and preparation method of solid-state battery
By constructing a multi-layer solid electrolyte structure on the solid-state battery electrode, the problem of insufficient interfacial contact in solid-state batteries has been solved, improving the cycle stability and safety of the battery, and enabling mass production.
Patent Information
- Application Number
- CN202411072423.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-10
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
In existing solid-state batteries, the interface contact between the solid electrolyte and the battery electrode is insufficient and the interface impedance is high, resulting in insufficient cycle stability and safety, and making it difficult to achieve mass production.
A multi-layer solid electrolyte structure is adopted, including an interface modification layer and an interface softening layer. A multi-layer composite electrode is constructed on the electrode sheet by high-pressure atomization spraying, which enhances the solid-solid contact area and interface compatibility, and reduces the interface impedance.
This improves lithium-ion transport rate, enhances the cycle stability and safety of solid-state batteries, and enables mass production.
Smart Images

Figure CN119008841A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of solid-state batteries and relates to a pole piece with a multi-layer solid-state electrolyte and a preparation method thereof, and a solid-state battery and a preparation method thereof. Background Art
[0002] As people's demand for the energy density of lithium-ion batteries continues to increase, improving the safety performance of lithium-ion batteries has attracted much attention. Currently, commercial lithium-ion batteries require the use of liquid organic electrolytes and diaphragms with poor thermal stability. As the operating temperature increases, the flammable and explosive liquid organic electrolytes and diaphragms that are easily shrunk and deformed by heat will seriously affect the safety of lithium-ion batteries.
[0003] Solid-state batteries use solid electrolytes instead of liquid electrolytes. Replacing flammable liquid electrolytes and separators with thermodynamically stable solid electrolytes can not only fundamentally solve the safety problems of lithium-ion batteries, but also simplify the manufacturing and packaging process, increase the freedom in battery structure design, and increase the energy density of the battery.
[0004] In the prior art, there are all-solid-state lithium-ion batteries using positive electrode composite materials with a core-shell structure, wherein the core layer includes a positive electrode active material, and the shell layer includes a polymer electrolyte and a sulfide solid electrolyte. This structural design improves the migration of lithium ions in the positive electrode material and the solid electrolyte, increases the ionic conductivity and electrochemical window of the shell solid electrolyte, and obtains an all-solid-state lithium-ion battery with better safety performance. However, the core-shell structure is unstable, and it is easy to have rapid capacity decay in the cycle stability test, and the battery rate is unstable, making it difficult to achieve mass production of solid-state battery pole pieces with stable structure.
[0005] There are also solid-state lithium batteries with multifunctional layered composite solid electrolytes in the prior art. The multifunctional layered composite solid electrolyte layer is located between the positive electrode and the negative electrode of the battery, and the composite solid electrolyte solution is evenly covered on the surface of the positive electrode collector and the negative electrode collector by a coating method. After secondary drying, a buffer electrolyte layer is obtained, and finally the main solid electrolyte layer is placed between the positive electrode and the negative electrode of the battery to form a solid-state battery, which increases the soft contact between the solid electrolyte and the battery pole piece and reduces the interface impedance in the solid-state battery to a certain extent. However, the thickness of the buffer electrolyte layer prepared by the coating method is uneven, the interface contact between the solid electrolyte and the battery pole piece is insufficient, and the interface impedance is still high. In addition, the process flow of the preparation process affects the stability of the solid electrolyte layer, causing the structure of the solid-state battery to be destroyed during the cycle, affecting the safety and cycle stability of the solid-state battery. Summary of the invention
[0006] Problem that the invention aims to solve
[0007] In view of the problems of insufficient interface contact between the above-mentioned solid electrolyte and the battery electrode, the need to further reduce the interface impedance, and the insufficient safety and cycle stability of the solid-state battery, there is an urgent need for an electrode and solid-state battery that can increase the solid-solid contact area, construct a flexible interface contact, have a stable structure, stable rate, excellent cycle performance and safety, as well as a preparation method that can improve the process effect of solid electrolyte introduction and solve the problem of mass production of solid-state battery electrodes.
[0008] Solutions for solving problems
[0009] In view of the above problems, the present invention provides a solid-state battery pole piece with multi-layer solid electrolytes. Through pole piece compounding and interface softening, the solid-solid contact interface can be improved, flexible interface contact can be provided, the lithium ion transmission rate can be increased, and the interface compatibility and cycle stability of the solid-state battery can be increased. In addition, the present invention also provides a method for preparing a solid-state battery pole piece with multi-layer solid electrolytes. The present invention adopts a high-pressure atomization spraying method to construct a solid-state battery pole piece with multi-layer solid electrolytes, which can achieve uniformity in the process of preparing layered composite pole pieces, can reduce interface impedance while improving the process effect of introducing solid electrolytes, construct a flexible solid-state battery interface, and improve the stability of the interlayer interface, solving the problem of mass production of solid-state battery pole pieces.
[0010] Specifically, the present invention provides a pole piece with a multi-layer solid electrolyte, which comprises: an interface modification layer and an interface softening layer sequentially arranged on a positive pole piece or a negative pole piece,
[0011] The interface softening layer comprises an organic polymer solid electrolyte and a lithium salt, and the interface modification layer comprises an interface modification material;
[0012] The interface modification layer can be partially filled into the interface softening layer and the electrode active material to form a filling layer containing the interface modification material and the solid electrolyte.
[0013] According to the pole piece described above, the pole piece having a multi-layer solid electrolyte further includes a second solid electrolyte layer on the interface softening layer.
[0014] According to the pole piece described above, the total thickness of the interface modification layer, the interface softening layer and the second solid electrolyte layer is 5 μm to 50 μm.
[0015] According to the above-mentioned pole piece, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium difluorooxalatoborate;
[0016] Preferably, in the interface softening layer, the mass ratio of the organic polymer solid electrolyte to the lithium salt is 2:1 to 8:1.
[0017] According to the pole piece described above, the solid electrolyte layer further includes an inorganic solid electrolyte.
[0018] According to the pole piece described above, the mass ratio of the organic polymer solid electrolyte to the inorganic solid electrolyte in the organic polymer solid electrolyte layer is 93:7 to 7:93.
[0019] According to the pole piece described above, the interface modification material comprises an inorganic ceramic material, and the inorganic ceramic material is selected from one or more of nitrides, carbides, metal oxides, non-metal oxides, and inorganic solid electrolytes;
[0020] Preferably, the inorganic ceramic material can be selected from one or more combinations of oxides, nitrides, borides, halides, carbides, dielectric ceramics, ferroelectric ceramics, piezoelectric ceramics, diatomaceous earth, mullite, montmorillonite and kaolin;
[0021] The oxides include, but are not limited to, one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate;
[0022] The nitride includes but is not limited to one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride;
[0023] The carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide, and niobium carbide;
[0024] The dielectric ceramics, ferroelectric ceramics and piezoelectric ceramics each include BaTiO 3 MgTiO 3 、CaTiO 3 PbTiO 3 、SrTiO 3 、BaO·TiO 2 、BaO-Nd 2 O 3 -TiO 2 、LiNbO 3 、LiTaO 3 、Cd 2 Ta 2 O 7 , Pb 2 Nb 2 O 7 、Cd2 Nb 2 O 7 , PbNb 2 O 6 , Sr 1-x Ba x Nb 2 O 6 , Ba 2 NeA 5 O 15 One or more of .
[0025] According to the pole piece described above, the second solid electrolyte used for the second solid electrolyte layer is selected from one or more of an inorganic solid electrolyte, an organic polymer solid electrolyte, and a lithium salt.
[0026] According to the pole piece described above, the inorganic solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte;
[0027] Preferably, the organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin;
[0028] According to the pole piece described above, the oxide solid electrolyte is selected from one or more of a garnet solid electrolyte, a perovskite solid electrolyte, a NASICON solid electrolyte and a LISICON solid electrolyte;
[0029] The garnet-type solid electrolyte includes Li x La 3 Zr y A z O 12 and / or Li x La 3-y B y Zr z O 12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga;
[0030] The perovskite solid electrolyte includes Li 3.3 La0.53 TiO 3 , Li 3x La 2 / 3-x TiO 3 and Li x Sr y M z TaO 3 One or more of; wherein M is one or more of Zr and Nb;
[0031] The NASICON-type solid electrolyte includes Li x Al y M z (PO 4 ) 3 , Li x Y y Zr z (PO 4 ) 3 、LiTi 2 (PO 4 ) 3 ,LiGe 2 (PO 4 ) 3 and LiGeTi(PO 4 ) 3 One or more of; wherein M is one or more of Ti, Ge, Hf, Zn, Zr, Si;
[0032] The LISICON type solid electrolyte includes Li 3+x (P 1-x Si x ) 4 and / or Li 3+x Ge x V 1-x O 4 ;
[0033] The sulfide solid electrolyte is selected from Argyrodite solid electrolyte LiPSMX, Thio-LiSICON solid electrolyte Li 4-x A 1-x B x S 4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga;
[0034] The glassy sulfide includes Li 2 S–P2 S 5 , Li 2 S–GeS 2 , Li 2 S-SiS 2 , Li 2 S-SiS 2 -Li 4 SiO 4 , Li 2 SB 2 S 3 , Li 2 SB 2 S 3 - one or more of LiI;
[0035] The halide solid electrolyte includes LiX, Li 2 MX 4、 Li 3 M′X 6 , Li x M″ y Ln z Cl 3、 LiM″′Cl 5 X″ and Li 3- y Zr y M″″ 1-y Cl 6 wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M′ is one or more of O, In, Y, Yb, Sc, Ho, Er, M″ is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M″′ is selected from one or more of La, Ta, Nb, X″ is selected from O, Cl, F or OH, and M″″ is selected from one or more of Y, Er, Yb, Ho, Lu;
[0036] Among them, 0 <x<1,0<y<1,0<z<1;
[0037] The borate solid electrolyte is selected from Li 2 B 4 O 7 , Li 2 OB 2 O 3 -P 2 O 5 One or more of;
[0038] The nitride solid electrolyte is selected from LiPON, Li 3 N.Li 7PN 4 、LiSi 2 N 3 One or more of;
[0039] The hydride solid electrolyte includes but is not limited to Li 3 AlH 6 , LiBH 4 、LiNH 2 , Li 2 NH, LiBH 4 -LiNH 2 , LiBH 4 -LiX; wherein X is one or more of Cl, Br or I;
[0040] Preferably, the perovskite-type oxide solid electrolyte is selected from lithium lanthanum titanium oxide;
[0041] The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide;
[0042] The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.
[0043] The present invention also provides a method for preparing the above-mentioned electrode sheet with multi-layer solid electrolyte, which comprises the following steps:
[0044] Step S2: spraying the slurry containing the interface modification material onto the surface of the positive electrode sheet or the negative electrode sheet by a high-pressure atomization spraying method to obtain a positive electrode sheet or a negative electrode sheet having an interface modification layer;
[0045] Step S4: spraying the slurry containing the organic polymer solid electrolyte onto the interface modification layer obtained in step S2 by a high-pressure atomization spraying method to obtain a positive electrode sheet or a negative electrode sheet having the interface modification layer and the interface softening layer; and
[0046] Optional step Sx: hot pressing the positive electrode sheet or the negative electrode sheet to partially fill the interface modification layer into the organic polymer solid electrolyte layer and the positive electrode sheet or the negative electrode sheet and form a filling layer containing the interface modification material and the organic polymer solid electrolyte.
[0047] According to the preparation method described above, the preparation method further comprises the following steps before step Sx:
[0048] Step S6: Spraying the slurry containing the second solid electrolyte onto the organic polymer solid electrolyte layer obtained in step S4 by a high-pressure atomization spraying method, thereby obtaining a positive electrode sheet or a negative electrode sheet of a multilayer solid electrolyte having the interface modification layer, the interface softening layer containing the organic polymer solid electrolyte and the second solid electrolyte layer.
[0049] According to the preparation method described above, the solid contents of the slurry containing the interface modification material, the slurry containing the organic polymer solid electrolyte and the slurry containing the second solid electrolyte are 5-80% by mass, preferably 10-60% by mass.
[0050] According to the preparation method described above, in the high-pressure atomization spraying method in step S2, step S4 and step S6, the spraying conditions are as follows: the pressure of the high-pressure pump is 10-30 MPa, the diameter of the nozzle is 0.5-3.0 mm, the spray width is 50-400 mm, the atomization pressure is 0.2-1.0 MPa, the spray flow rate is 50-450 mL / min, the spray distance is 20-350 mm, and the spray angle is 80-93°;
[0051] Preferably, the spraying conditions in step S2, step S4 and step S6 are the same or different.
[0052] According to the preparation method described above, the slurry in step S2 further comprises one or more of a conductive agent and a binder;
[0053] Preferably, the slurry in step S4 further comprises an inorganic solid electrolyte;
[0054] Preferably, the slurry in step S4 and the slurry in step S6 each further comprise a binder;
[0055] Preferably, when the second solid electrolyte in step S6 includes only an organic polymer solid electrolyte, the slurry in step S6 includes a lithium salt.
[0056] According to the preparation method described above, the positive electrode active material described in the present invention includes but is not limited to one or more combinations of nickel-cobalt-manganese ternary materials, nickel-cobalt-aluminum ternary materials, lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium vanadium phosphate, and lithium-rich manganese-based materials.
[0057] The negative electrode active materials described in the present invention include but are not limited to one or more combinations of graphite, graphene, soft carbon, hard carbon, elemental silicon, silicon-oxygen materials, silicon-carbon materials, silicon-nitrogen composite materials, silicon-based alloys, elemental tin, tin oxide compounds, tin-based alloys, lithium metal, lithium alloy negative electrode, lithium titanium oxide, transition metal oxides and transition metal sulfides.
[0058] The conductive agent of the present invention is selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon nanofibers, carbon molecular sieves, polyethylene dioxythiophene, polystyrene sulfonic acid and lithium polystyrene sulfonate;
[0059] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium difluorooxalatoborate;
[0060] Preferably, the binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate;
[0061] Preferably, the binder contained in the slurry in step S2, the slurry in step S2 and the slurry in step S6 are the same as or different from each other;
[0062] Preferably, the slurry in step S4 and the lithium salt contained in the slurry in step S4 are the same or different.
[0063] According to the preparation method described above, in the hot pressing of step Sx, the hot pressing temperature is 40-60° C., the pressure is 0.1-0.5 MPa, and the hot pressing time is 5-20 minutes.
[0064] The present invention also provides a solid-state battery, which includes the pole piece described above or the pole piece obtained by the preparation method described above.
[0065] The present invention further provides a method for preparing a solid-state battery, comprising:
[0066] The step of preparing a positive electrode sheet and / or a negative electrode sheet having a multilayer solid electrolyte by the preparation method described above; and
[0067] The positive electrode sheet and the negative electrode sheet are stacked and packaged, and then optionally hot-pressed and integrated after packaging.
[0068] According to the preparation method described above, in the hot pressing integration, the hot pressing temperature is 50-80° C., the pressure is 0.2-0.8 MPa, and the hot pressing time is 20-40 minutes.
[0069] Effects of the Invention
[0070] The technical solution of the present invention has the following beneficial effects:
[0071] (1) The present invention provides a solid-state battery pole piece with a multilayer solid electrolyte such as an interface modification layer and an interface softening layer, wherein the interface modification layer increases the solid-solid contact area between the solid electrolyte and the electrode active material, improves the electron / ion transmission channel, and improves the interface compatibility. The organic polymer solid electrolyte provides a flexible solid-state battery interface. The multilayer interface is in close contact through the pole piece composite and the interface softening, further reducing the interface impedance, thereby achieving the replacement of the diaphragm, constructing a stable solid-state battery interface, and improving the cycle stability of the solid-state battery;
[0072] (2) The present invention uses a high-pressure atomization spraying method to prepare a solid-state battery electrode sheet with a multi-layer solid electrolyte, ensure the uniformity of the multi-layer structure, prevent the agglomeration of tiny solute particles during the introduction of the slurry, and achieve uniform preparation of a battery electrode sheet containing a multi-layer solid electrolyte while accurately controlling the thickness of each solid electrolyte layer, thereby improving the energy density of the solid-state battery and greatly improving the production efficiency, thereby realizing mass production of solid-state batteries;
[0073] (3) The present invention adopts a high-pressure atomization spraying method to ensure that the electrode active material is in full contact with the solid electrolyte during the electrode composite process, thereby solving the solid-solid contact problem, increasing the contact area between the solid electrolyte and the battery electrode, reducing the interface resistance, and improving the lithium ion transmission rate. By softening the interface and slowly releasing the interface stress, a stable multi-layer solid interface is constructed, thereby improving the electrochemical performance and safety of the solid-state battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 1 is a graph showing the first charge and discharge curve of the multilayer composite electrode prepared in Example 1 of the present invention.
[0075] Figure 2 is a scanning electron microscope characterization image showing the battery electrode prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0076] The following describes the embodiments of the present invention, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope of the invention claim, and the embodiments obtained by appropriately combining different embodiments and appropriately combining the technical means disclosed in the embodiments are also included in the technical scope of the present invention. In addition, all the documents recorded in this specification are cited in this specification as references.
[0077] Unless defined otherwise, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0078] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0079] In this specification, unless otherwise specified, "multiple" in "multiple", "multiple", "plurality", etc. means a numerical value of 2 or more.
[0080] In the present specification, the term “substantially”, “substantially” or “essentially” means that the error is less than 5%, less than 3%, or less than 1% compared with a relevant perfect standard or theoretical standard.
[0081] In this specification, unless otherwise specified, "%" means mass percentage.
[0082] In this specification, if "room temperature", "normal temperature" or the like appears, the temperature may generally be 10 to 37°C, or 15 to 35°C.
[0083] In this specification, the meanings of “may” or “can” include both existence and non-existence, and both performing a certain process and not performing a certain process.
[0084] As used herein, “optional” and “optionally” mean that the subsequently described event or circumstance may or may not occur, and that the description includes instances where the event occurs and instances where it does not occur.
[0085] The term "comprising" and any variations thereof in the specification and claims of the present invention and the above drawings are intended to cover non-exclusive inclusions. For example, a process, method or system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.
[0086] In this specification, the references to "some / certain / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0087] In solid-state lithium-ion batteries, structural design is required to achieve good interface contact between the solid electrolyte layer and the positive and negative active materials, improve the solid interface stability, and reduce solid-solid poor contact. A reasonable structure can increase the contact area of active materials in solid-state batteries, thereby improving the utilization of positive and negative active materials and solid electrolytes. At the same time, in order to avoid the influence of disordered structures on energy density and charging performance in solid-state batteries and improve the transmission rate of lithium ions in solid-state batteries, a reasonable battery structure can effectively improve the electrochemical performance and energy density of solid-state batteries. The structural design of solid-state batteries needs to comprehensively consider the manufacturing processes of the positive and negative electrodes, as well as the introduction process of solid-state electrolytes and the manufacturing process of battery pole pieces containing solid-state electrolytes.
[0088] Different from the button batteries used in the laboratory, the rational design of the solid-state battery structure and its application in the battery cell requires overcoming many process manufacturing difficulties, which is the most critical factor in breaking through the industrial application of solid-state batteries. Compared with the manufacturing process of traditional lithium-ion batteries, including rolling and coating, directly introducing solid-state batteries into the manufacturing process will also cause the internal structure of the electrode to expand and deform, the pole piece to pulverize, and thus increase the resistance, which in turn affects the battery's cycle performance.
[0089] Therefore, designing a reasonable structure and developing a manufacturing process that is more suitable for solid-state batteries are of great value in the research in the field of solid-state batteries. Only by using solid-state battery manufacturing process methods and processes that can build multi-layer battery structures can the leap from theory to actual mass production of solid-state batteries be realized.
[0090] The pole piece with multi-layer solid electrolyte and its preparation method, the solid-state battery and its preparation method of the present invention are described in detail below.
[0091] <First aspect>
[0092] The first aspect of the present invention relates to a pole piece with a multi-layer solid electrolyte, comprising: an interface modification layer and an interface softening layer sequentially arranged on a positive pole piece or a negative pole piece by pole piece composite,
[0093] The interface softening layer comprises an organic polymer solid electrolyte and a lithium salt, and the interface modification layer comprises an interface modification material;
[0094] The interface modification layer can be partially filled into the interface softening layer and the electrode active material to form a filling layer containing the interface modification material and the solid electrolyte.
[0095] In the present invention, the interface softening layer can provide a flexible interface, avoid gaps caused by solid-solid interface contact and point contact, increase the interface contact area, and improve the interlayer flexible contact and interface compatibility.
[0096] In the present invention, an interface modification layer is added between the interface of the positive electrode plate or the negative electrode plate and the interface softening layer, wherein the interface modification layer is different from the interface softening layer and the second solid electrolyte layer, and is also different from the solid electrolyte layer in other conventional technologies, and its performance and function are significantly different from the interface softening layer and the second solid electrolyte layer. The ion conductivity of the interface modification layer is lower than that of the second solid electrolyte layer. The function of the interface modification layer is to fill the interface gap in the solid-state battery, reduce the interface impedance, increase the transmission rate of lithium ions between the interfaces, prevent the occurrence of interface side reactions, and improve the cycle stability of the solid-state battery.
[0097] In addition, by providing an interface modification layer, the solid electrolyte can be prevented from directly contacting the positive electrode layer or the negative electrode layer, thereby preventing some solid electrolytes from reacting with the positive electrode or the negative electrode and reducing the cycle stability of the battery. In addition, compared with directly adding the interface modification material to the interface softening layer, the agglomeration and uneven dispersion of the interface modification material particles during the mixing or drying process can be avoided, preventing the battery from short-circuiting. Adding an interface modification layer alone can avoid direct contact between the flexible interface of the organic polymer solid electrolyte layer and the positive electrode sheet or the negative electrode sheet, increase the cycle stability under high voltage, and the separate interface modification layer is in close contact with the positive electrode side, providing a stable channel for the transmission of lithium ions and electrons.
[0098] In some preferred embodiments of the present invention, the interface modification layer can be partially filled into the interface softening layer to form a filling layer containing an interface modification material and a solid electrolyte. The filling layer increases the interface contact between the flexible interface of the organic polymer solid electrolyte layer and the interface modification layer, increases the compatibility between the solid interfaces, thereby reducing the crystallization area of the polymer, inducing ion transmission behavior and forming a new ion transmission interface, improving the electrochemical stability window of the solid electrolyte, improving the ionic conductivity between the multilayer structure, and increasing the compatibility of the electrode and the solid electrolyte interface.
[0099] The organic polymer solid electrolyte layer of the present invention contains a lithium salt, which can be selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium difluorooxalate borate. In the organic polymer solid electrolyte layer, the mass ratio of the organic polymer solid electrolyte to the lithium salt can be 2:1 to 8:1, for example, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, etc.
[0100] In some preferred embodiments of the present invention, an inorganic solid electrolyte is also included in the organic polymer solid electrolyte layer. The mass ratio of the organic polymer solid electrolyte to the inorganic solid electrolyte in the organic polymer solid electrolyte layer may be 93:7 to 7:93, for example, 93:7, 90:10, 80:20, 70:30, 60:40, 50:50, 40:60, 30:70, 20:80, 10:90, 7:93, etc.
[0101] In some preferred embodiments of the present invention, the electrode having a multi-layer solid electrolyte further comprises a second solid electrolyte layer on the organic polymer solid electrolyte layer.
[0102] The total thickness of the interface modification layer, the interface softening layer and the second solid electrolyte layer is 5 μm to 50 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc. Their total thickness within the above range can effectively separate the positive electrode and the negative electrode, and ensure the cycle stability of the solid-state battery under the premise of ensuring the battery energy density. Too low thickness will lead to interface failure during the cycle, and the contact between the positive and negative electrodes will cause a short circuit; too high thickness will increase the internal resistance of the battery, increase the cost, and is not conducive to the design of high energy density battery cells.
[0103] The thickness of the interface modification layer may be 500nm to 10μm, for example, 500nm, 800nm, 1μm, 2μm, 5μm, 10μm, etc. The thickness of the interface modification layer within this range can effectively increase the interlayer interface contact, build a flexible interface, reduce the interlayer interface impedance, and improve the cycle stability of the composite electrode.
[0104] The thickness of the interface softening layer may be 5 μm to 30 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, etc.
[0105] The thickness of the second solid electrolyte layer may be 5 μm to 40 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, etc.
[0106] In the present invention, the interface modification material includes an inorganic ceramic material, and the inorganic ceramic material can be selected from one or more of nitrides, carbides, metal oxides, non-metal oxides, and inorganic solid electrolytes.
[0107] Specifically, the oxide includes, but is not limited to, one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate;
[0108] Specifically, the nitride includes, but is not limited to, one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride;
[0109] Specifically, the carbide is selected from one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide, and niobium carbide;
[0110] Specifically, the dielectric ceramic, the ferroelectric ceramic, and the piezoelectric ceramic each contain BaTiO 3 MgTiO 3 、CaTiO 3 PbTiO 3 、SrTiO 3 、BaO·TiO 2 、BaO-Nd 2 O 3 -TiO 2 、LiNbO 3 、LiTaO 3 、Cd 2 Ta 2 O 7 , Pb 2 Nb 2 O 7 、Cd 2 Nb 2 O 7 , PbNb 2 O 6 , Sr 1-x Ba x Nb 2 O 6 , Ba 2 NeA 5 O 15 One or more of;
[0111] Selecting nitrides as interface modification materials can improve the thermal stability and safety of solid-state batteries. The low density of nitrides can effectively reduce the quality of the batteries and control production costs.
[0112] In the present invention, the organic polymer solid electrolyte for the organic polymer solid electrolyte layer can be selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polycyanoethyl acrylate, polypentylene succinate, polyvinyl chloride, polyvinylene carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin. When two or more organic polymer solid electrolytes are used, the ratio between them is not particularly limited and can be adjusted according to actual needs.
[0113] In the present invention, the second solid electrolyte used for the second solid electrolyte layer is selected from one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte. Among them, it is preferred to use a composite solid electrolyte of an inorganic solid electrolyte and an organic polymer solid electrolyte at the same time, and the composite solid electrolyte layer can further improve the interfacial compatibility and the cycle stability of the battery. When the second solid electrolyte includes both an inorganic solid electrolyte and an organic polymer solid electrolyte, the ratio between them is not particularly limited. For example, the mass ratio of the inorganic solid electrolyte to the organic polymer solid electrolyte can be 20:1 to 5:1, preferably 15:1 to 10:1.
[0114] The inorganic solid electrolyte may be selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte.
[0115] Examples of the organic polymer solid electrolyte are the same as those listed in the organic polymer solid electrolyte for the organic polymer solid electrolyte layer, and may be the same as or different from the organic polymer solid electrolyte for the organic polymer solid electrolyte layer.
[0116] In the present invention, the oxide solid electrolyte is selected from one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, a NASICON-type solid electrolyte and a LISICON-type solid electrolyte;
[0117] Garnet-type solid electrolytes include Li x La 3 Zr y A z O 12 and / or Li x La 3-y B y Zr z O 12; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga;
[0118] Perovskite solid electrolytes include Li 3.3 La 0.53 TiO 3 , Li 3x La 2 / 3-x TiO 3 and Li x Sr y M z TaO 3 One or more of; wherein M is one or more of Zr and Nb;
[0119] NASICON-type solid electrolytes include Li x Al y M z (PO 4 ) 3 , Li x Y y Zr z (PO 4 ) 3 、LiTi 2 (PO 4 ) 3 ,LiGe 2 (PO 4 ) 3 and LiGeTi(PO 4 ) 3 One or more of; wherein M is one or more of Ti, Ge, Hf, Zn, Zr, Si;
[0120] LISICON type solid electrolyte includes Li 3+x (P 1-x Si x ) 4 and / or Li 3+x Ge x V 1-x O 4 ;
[0121] The sulfide solid electrolyte is selected from Argyrodite-type solid electrolyte LiPSMX, Thio-LiSICON-type solid electrolyte Li 4-x A 1-x B x S 4and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga;
[0122] Glassy sulfides include Li 2 S–P 2 S 5 , Li 2 S–GeS 2 , Li 2 S-SiS 2 , Li 2 S-SiS 2 -Li 4 SiO 4 , Li 2 SB 2 S 3 , Li 2 SB 2 S 3 - one or more of LiI;
[0123] Halide solid electrolytes include LiX, Li 2 MX 4、 Li 3 M′X 6 , Li x M″ y Ln z Cl 3、 LiM″′Cl 5 X″ and Li 3- y Zr y M″″ 1-y Cl 6 wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M′ is one or more of O, In, Y, Yb, Sc, Ho, Er, M″ is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M″′ is selected from one or more of La, Ta, Nb, X″ is selected from O, Cl, F or OH, and M″″ is selected from one or more of Y, Er, Yb, Ho, Lu;
[0124] Among them, 0 <x<1,0<y<1,0<z<1;
[0125] The borate solid electrolyte is selected from Li 2 B 4 O7 , Li 2 OB 2 O 3 -P 2 O 5 One or more of;
[0126] The nitride solid electrolyte is selected from LiPON, Li 3 N.Li 7 PN 4 、LiSi 2 N 3 One or more of;
[0127] Hydride solid electrolytes include but are not limited to Li 3 AlH 6 , LiBH 4 、LiNH 2 , Li 2 NH, LiBH 4 -LiNH 2 , LiBH 4 -LiX; wherein X is one or more of Cl, Br or I;
[0128] Preferably, the perovskite oxide solid electrolyte is selected from lithium lanthanum titanium oxide;
[0129] The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide;
[0130] The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.
[0131] <Second Aspect>
[0132] A second aspect of the present invention relates to a method for preparing a pole piece having a multilayer solid electrolyte, comprising the following steps:
[0133] Step S2: spraying the slurry containing the interface modification material onto the surface of the positive electrode sheet or the negative electrode sheet by a high-pressure atomization spraying method to obtain a positive electrode sheet or a negative electrode sheet having an interface modification layer;
[0134] Step S4: spraying the slurry containing the organic polymer solid electrolyte onto the interface modification layer obtained in step S2 by a high-pressure atomization spraying method to obtain a positive electrode sheet or a negative electrode sheet having the interface modification layer and the interface softening layer; and
[0135] Optional step Sx: hot pressing the positive electrode sheet or the negative electrode sheet to partially fill the interface modification layer into the organic polymer solid electrolyte layer and the positive electrode sheet or the negative electrode sheet and form a filling layer containing the interface modification material and the solid electrolyte.
[0136] In some preferred embodiments, the preparation method of the present invention may further include the following steps before step Sx:
[0137] Step S6: Spraying the slurry containing the second solid electrolyte onto the polymer solid electrolyte layer obtained in step S4 by a high-pressure atomization spraying method, thereby obtaining a positive electrode sheet or a negative electrode sheet of a multilayer solid electrolyte having the interface modification layer, the interface softening layer containing the organic polymer solid electrolyte and the second solid electrolyte layer.
[0138] In addition, the preparation method of the present invention may further include the step of preparing a slurry, for example, the following steps may be included:
[0139] Step S1: homogenizing a composition containing an interface modification material in an organic solvent to prepare a slurry containing the interface modification material; and / or
[0140] Step S3: homogenizing the composition containing the organic polymer solid electrolyte and the lithium salt in an organic solvent to prepare a slurry containing the organic polymer solid electrolyte.
[0141] In some preferred embodiments, the preparation method of the present invention may further include the following slurry preparation steps:
[0142] Step S5: slurrying the composition containing the second solid electrolyte in an organic solvent to prepare a slurry containing the second solid electrolyte.
[0143] In the present invention, there is no particular limitation on the preparation method of the positive electrode sheet or the negative electrode sheet, and the positive electrode sheet can be prepared by using common methods in the art such as traditional coating method, dry electrostatic spraying method, wet electrostatic spraying method, etc.
[0144] Each step is described in detail below.
[0145] Step S1
[0146] In step S1 , a composition containing an interface modification material is slurried in an organic solvent to prepare a slurry containing the interface modification material.
[0147] Examples of the interface modification material used in step S1 are the same as the examples of the interface modification material listed in the above <First Aspect>, and will not be repeated here.
[0148] In the present invention, the solid content of the slurry containing the interface modification material can be 5-80 mass%, preferably 10-60 mass%, for example, 5 mass%, 10 mass%, 15 mass%, 20 mass%, 30 mass%, 40 mass%, 50 mass%, 60 mass%, 70 mass%, 80 mass%, etc. The solid content within the above range is conducive to the spraying and uniform distribution of the interface modification material, and prevents the process problem of material jamming during high-pressure atomization spraying due to too high concentration, and prevents the process problem of active material agglomeration during high-pressure atomization spraying due to too low concentration, which affects the distribution of the interface modification material on the battery pole piece.
[0149] In step S1, the organic solvent used in homogenization can be selected from one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide, butyrate, toluene, xylene, anisole, hexane, heptane, dibromomethane, dichloroethane, ethanol and glycol ether.
[0150] In some preferred embodiments, the composition containing the interface modification material in step S1 further comprises a conductive agent and a binder.
[0151] The present invention does not particularly limit the conductive agent and the binder, and those commonly used in the art can be used. For example, the conductive agent can be selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon nanofibers, carbon molecular sieves, polyethylene dioxythiophene, polystyrene sulfonic acid and lithium polystyrene sulfonate. The binder can be selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate.
[0152] In some specific embodiments of the present invention, during homogenization, the interface modification material, the optional conductive agent and the optional binder may be uniformly mixed in a ball mill, and then a solvent is added and stirred to prepare a slurry with a desired solid content.
[0153] Step S2
[0154] In step S2, the slurry containing the interface modification material prepared in step S1 is sprayed onto the surface of the positive electrode sheet or the negative electrode sheet by a high-pressure atomization spraying method, thereby obtaining a positive electrode sheet or a negative electrode sheet having an interface modification layer.
[0155] In the present invention, during the high-pressure atomization spraying in step S2, the atomization pressure can be 0.2-1.0MPa, preferably 0.25-0.8MPa, for example, 0.2MPa, 0.25MPa, 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, 0.7MPa, 0.8MPa, 0.9MPa, 1.0MPa, etc. When the pressure of the high-pressure atomization is within the above range, the slurry can be evenly sprayed on the surface of the battery pole piece, which is conducive to controlling the thickness of the obtained interface modification layer and increasing the effective adsorption rate of the interface modification material slurry. Too low atomization pressure will lead to uneven distribution of the interface modification material sprayed on the surface of the battery pole piece and affect the interface contact between the solid electrolyte layer and the battery pole piece.
[0156] In addition, the spraying conditions in the high pressure atomization spraying of the present invention also include the following:
[0157] The pressure of the high-pressure pump is 10-30 MPa, for example, 10 MPa, 15 MPa, 20 MPa, 25 MPa, 30 MPa, etc.;
[0158] The diameter of the nozzle is 0.5 to 3.0 mm, for example, 0.5 mm, 1.0 mm, 1.5 mm, 2.0 mm, 2.5 mm, 3.0 mm, etc.;
[0159] The carrier gas flow rate is controlled to be 50-350 L / min, for example, 50 L / min, 100 L / min, 150 L / min, 200 L / min, 250 L / min, 300 L / min, 350 L / min, etc.;
[0160] The spraying rate of the slurry is 50 to 450 mL / min, for example, 50 mL / min, 100 mL / min, 150 mL / min, 200 mL / min, 250 mL / min, 300 mL / min, 350 mL / min, 400 mL / min, 450 mL / min, etc.
[0161] The spray width is 50-400 mm, for example, 50 mm, 100 mm, 120 mm, 150 mm, 180 mm, 200 mm, 230 mm, 300 mm, 320 mm, 350 mm, 400 mm, etc. The spray width within this range can improve the uniformity of the spraying process, prevent blockage and uneven thickness of the prepared electrolyte layer, and improve production efficiency.
[0162] The spraying distance between the target battery pole piece and the high-pressure atomization equipment can be 20 to 350 mm, preferably 50 to 300 mm, for example, it can be 20 mm, 30 mm, 50 mm, 60 mm, 80 mm, 100 mm, 120 mm, 150 mm, 180 mm, 200 mm, 250 mm, 300 mm, 350 mm, etc.
[0163] The spraying angle may be 80° to 93°, for example, 80°, 85°, 88°, 90°, 93°, etc.
[0164] Selecting a nozzle diameter and a spray flow rate within the above range can reduce the problems of agglomeration of interface modification material particles and slurry waste, improve the control accuracy and atomization effect during the spraying process, and increase the spraying efficiency.
[0165] In addition, the high-pressure atomization spraying of the present invention is preferably carried out in a dry environment with a moisture content of less than 10 ppm, preferably 5 ppm, and more preferably less than 1 ppm.
[0166] In some preferred embodiments of the present invention, the positive electrode sheet or the negative electrode sheet can be heated. The heating temperature can be 55-205°C, preferably 75-155°C, for example, 55°C, 60°C, 70°C, 75°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 155°C, 160°C, 170°C, 180°C, 190°C, 200°C, 205°C, etc. By heating the electrode sheet, the electrolyte slurry can be evenly distributed on the surface of the electrode sheet, the agglomeration of the solid electrolyte during the mixing process can be reduced, and the cycle stability of the battery can be improved.
[0167] In some embodiments, the positive electrode sheet or the negative electrode sheet is placed on a working plate for operation. Thus, the temperature of the positive electrode sheet or the negative electrode sheet can be increased through the working plate, thereby achieving mass production while reducing the process flow.
[0168] In some specific embodiments, the positive electrode sheet or the negative electrode sheet is placed on a working plate, which is then heated and spraying conditions are set, and a slurry containing an interface modification material is sprayed onto the surface of the sheet to a desired thickness. After standing for a period of time, the static coating equipment is turned off, and the sheet is then cooled naturally, thereby obtaining a positive electrode sheet or a negative electrode sheet with an interface modification layer.
[0169] In some embodiments, during the standing period, the temperature of the working plate may be raised to a temperature slightly higher than the heating temperature during spraying, for example, 10 to 30° C. higher. The standing period may be, for example, 20 to 120 minutes.
[0170] In some embodiments of the present invention, the thickness of the interface modification layer may be 500nm to 10μm, for example, 500nm, 800nm, 1μm, 2μm, 5μm, 10μm, etc. The thickness of the interface modification layer within this range can effectively increase the interlayer interface contact, construct a flexible interface and reduce the interlayer interface impedance, thereby improving the cycle stability of the composite electrode.
[0171] Step S3
[0172] In step S3 , the composition containing the organic polymer solid electrolyte and the lithium salt is slurried in an organic solvent to prepare a slurry containing the organic polymer solid electrolyte.
[0173] The examples and proportions of the organic polymer solid electrolyte and the lithium salt used in step S3 are the same as the examples and proportions of the organic polymer solid electrolyte listed in the above <First Aspect>, and are not repeated here.
[0174] In the present invention, the solid content of the slurry containing the organic polymer solid electrolyte can be 5-80% by mass, preferably 10-60% by mass, for example, 5%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80% by mass, etc. The solid content within the above range is conducive to the ejection and uniform distribution of the organic polymer solid electrolyte, and prevents the process problem of material jamming during high-pressure atomization spraying due to too high concentration, and prevents the process problem of powder falling during high-pressure atomization spraying due to too low concentration, which affects the distribution of the organic polymer solid electrolyte.
[0175] In step S3, examples of the organic solvent used in the homogenization are the same as those in step S1 above. In a specific embodiment, the organic solvent used in step S3 may be the same as or different from that in step S1. In addition, a dispersant may also be added during the homogenization. The present invention does not particularly limit the dispersant, and a dispersant commonly used in the art can be used.
[0176] In some preferred embodiments, the composition of the organic polymer solid electrolyte in step S3 further comprises an inorganic solid electrolyte. Examples of the inorganic solid electrolyte are the same as those listed in the above <First Aspect>.
[0177] In some preferred embodiments, the composition containing the polymer solid electrolyte in step S3 may further contain a binder.
[0178] There is no particular limitation on the binder, and those commonly used in the art can be used. In some embodiments of the present invention, examples of the binder are the same as those listed in step S1 above, and in a specific embodiment, the binder used in step S3 can be the same or different from that in step S1.
[0179] In step S3, when preparing the slurry, the organic polymer solid electrolyte and lithium salt etc. can be sequentially added into the solvent and stirred at 50-80°C for 5-12 hours to mix evenly, and a dispersant can be added to obtain a slurry with a desired solid content.
[0180] Step S4
[0181] In step S4, the slurry containing the organic polymer solid electrolyte prepared in step S3 is sprayed onto the interface modification layer obtained in step S2 by a high-pressure atomization spraying method, thereby obtaining a positive electrode sheet or a negative electrode sheet having an interface modification layer and an organic polymer solid electrolyte layer in sequence.
[0182] The range of each condition of high pressure atomization spraying in step S4 is the same as that in step S2 above, and will not be repeated here. In a specific embodiment, the conditions of high pressure atomization spraying adopted in step S4 may be the same as or different from those in step S2.
[0183] In addition, in step S4, the high-pressure atomization spraying is preferably performed in a dry environment with a moisture content of less than 5 ppm, preferably less than 1 ppm.
[0184] Step S5
[0185] In some preferred embodiments of the present invention, the method for preparing a pole piece may further include step S5: slurrying a composition containing a second solid electrolyte and an optional lithium salt in an organic solvent to prepare a slurry containing the second solid electrolyte.
[0186] In the present invention, there is no particular limitation on the second solid electrolyte, and those commonly used in the art can be used.
[0187] In some embodiments of the present invention, the second solid electrolyte may be selected from one or more of an inorganic solid electrolyte and an organic polymer solid electrolyte. Examples of the inorganic solid electrolyte and the organic polymer solid electrolyte are the same as those listed in the above <First Aspect>.
[0188] In step S5, examples of the organic solvent used in the homogenization are the same as those listed in step S1, and may be the same as or different from the organic solvents used in step S1 and step S3. A dispersant may also be added during the homogenization. The present invention does not particularly limit the dispersant, and a dispersant commonly used in the art may be used.
[0189] In the present invention, the solid content of the slurry containing the second solid electrolyte may be 5% to 80% by mass, preferably 10 to 60% by mass, for example, 5%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80% by mass, etc. The solid content within the above range is conducive to the ejection and uniform distribution of the second solid electrolyte, and prevents the process problem of material jamming during high-pressure atomization spraying due to excessively high concentration, and prevents the process problem of powder falling during high-pressure atomization spraying due to too low concentration, which affects the distribution of the solid electrolyte.
[0190] When the second solid electrolyte in step S5 includes only an organic polymer solid electrolyte, the composition in step S5 includes a lithium salt. Examples and amounts of the lithium salt are the same as those listed in step S3, and in a specific embodiment, the lithium salt used in step S5 may be the same as or different from that used in step S3.
[0191] In some preferred embodiments, the composition containing the second solid electrolyte in step S5 further contains a binder. Examples of the binder are the same as those listed in step S3, and in a specific embodiment, the binder used in step S5 may be the same as or different from that used in step S3.
[0192] Step S6
[0193] In step S6, the slurry containing the second solid electrolyte prepared in step S5 is sprayed onto the organic polymer solid electrolyte layer obtained in step S4 by high-pressure atomization spraying, thereby obtaining a positive electrode sheet or a negative electrode sheet having a multilayer solid electrolyte having an interface modification layer, an organic polymer solid electrolyte layer and a second solid electrolyte layer in sequence.
[0194] The range of each condition of high pressure atomization spraying in step S6 is the same as that in step S2 above, and will not be repeated here. In a specific embodiment, the conditions of high pressure atomization spraying adopted in step S6 may be the same as or different from those in step S2 and step S4.
[0195] Step Sx
[0196] In step Sx, the finally prepared positive electrode sheet or negative electrode sheet is hot pressed, so that the interface modification layer is partially filled into the organic polymer solid electrolyte layer and a filling layer containing the interface modification material and the organic polymer solid electrolyte is formed.
[0197] Since no drying is performed after the spraying step before step Sx, a filling layer in which the organic polymer solid electrolyte layer is partially filled with the interface modification layer is automatically formed by the hot pressing step.
[0198] In the electrode sheet preparation method of the present invention, step Sx is performed optionally. In the subsequent solid-state battery preparation process, after the positive and negative electrode sheets are stacked and packaged, a hot pressing integration step is required, which will also cause the interface modification layer to partially fill the organic polymer solid electrolyte layer to form a filling layer. It is preferred to perform step Sx, thereby further reducing the interface impedance.
[0199] In the hot pressing of the present invention, the hot pressing temperature can be 40 to 60°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, etc., the pressure can be 0.1 to 0.5 MPa, for example, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, etc., and the hot pressing time can be 5 to 20 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, etc.
[0200] During the hot pressing process, the interface contact between the flexible interface of the organic polymer solid electrolyte layer and the interface modification layer is increased to form a filling layer containing the interface modification material and the organic polymer solid electrolyte. The crystallization area of the polymer is reduced on the basis of reducing the process steps, inducing ion transport behavior and forming a new ion transport interface, thereby improving the electrochemical stability window of the solid electrolyte, improving the ionic conductivity between the multilayer structure, and increasing the compatibility of the electrode and the solid electrolyte interface.
[0201] In the preparation method of the present invention, by regulating the physical properties of each solid electrolyte slurry and the process parameters of the high-pressure atomization spraying device, the slurry containing the solid electrolyte meets the requirements of the high-pressure atomization spraying, and the process problems such as material sticking and clogging caused by the agglomeration and sedimentation of the solid electrolyte are improved, the production efficiency is greatly improved and the equipment maintenance cost is reduced. The atomization effect is good and the control accuracy is high, and a continuous and dense solid electrolyte layer can be directly constructed on the battery electrode, the interface contact between the electrode and the solid electrolyte layer is enhanced, and the interface impedance is reduced, thereby improving the electrochemical performance of the solid-state battery.
[0202] The present invention uses a high-pressure atomization spraying method to prevent the agglomeration of tiny solute particles in the slurry during the introduction process, thereby achieving uniform preparation of battery pole pieces containing solid electrolytes while accurately controlling the thickness of the solid electrolyte layer and improving the energy density of the solid-state battery; the present invention solves the problem of mass production of battery pole pieces containing solid electrolytes through high-pressure atomization spraying and improves production efficiency.
[0203] <Third Aspect>
[0204] The third aspect of the present invention relates to a solid-state battery, which includes the pole piece in the above <first aspect> or the pole piece obtained by the preparation method described in the above <second aspect>.
[0205] <Fourth Aspect>
[0206] The fourth aspect of the present invention relates to a method for preparing a solid-state battery, comprising: preparing a positive electrode sheet and / or a negative electrode sheet having a multilayer solid electrolyte by the preparation method described in the above <Second Aspect>; and
[0207] The steps of packaging the positive electrode sheets and / or the negative electrode sheets and then hot pressing them for integration.
[0208] In the hot pressing integration of the present invention, the hot pressing temperature can be 50-80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc., the pressure can be 0.2-0.8MPa, for example, 0.2MPa, 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, 0.7MPa, 0.8MPa, etc., and the hot pressing time can be 20-40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.
[0209] Example
[0210] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0211] Example 1
[0212] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0213] (1) Aluminum nitride, conductive carbon black, and polyvinylidene fluoride were mixed uniformly in a ball mill at a mass ratio of 8:1:1, and the speed was set at 200 r / min for 3 hours. The mixture was added to DMF solvent to prepare a slurry with a solid content of 40% by mass, and the mixture was fully stirred for 6 hours;
[0214] (2) The above slurry is sprayed on the lithium iron phosphate positive electrode sheet by high-pressure atomization spraying (positive electrode active material lithium iron phosphate (LiFePO4), conductive carbon black (SP), and adhesive polyvinylidene fluoride (PVDF) are dispersed in solvent N-methylpyrrolidone (NMP) and mixed evenly to obtain positive electrode slurry, wherein the mass ratio of lithium iron phosphate, PVDF and conductive carbon black is 94:3:3. The positive electrode slurry is coated on aluminum foil, and after drying and rolling, a positive electrode sheet is obtained.
[0215] Set the spray distance to 200mm, the spray angle to 90°, the nozzle diameter to 2.0mm, the high-pressure pump pressure to 25MPa, the atomization pressure to 0.3MPa, and the spray flow rate to 100
[0216] mL / min, spray width 300mm, to obtain an interface modification layer containing the interface modification material with a thickness of 5 μm;
[0217] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0218] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the lithium iron phosphate positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0219] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0220] (5) Li 7 La 3 Zr 2 O 12 The solid electrolyte was dissolved in DMF solvent, stirred thoroughly and added with dispersant. After sand milling for 2 hours, the obtained solution was 7 La 3 Zr 2 O 12 , polyvinylidene fluoride, and polypentylene succinate in a mass ratio of 23:1:1, adding polyvinylidene fluoride and polypentylene succinate to prepare a slurry with a solid content of 60% by mass;
[0221] (6) Use high-pressure atomization spray to coat Li 7 La 3 Zr 2 O 12 The solid electrolyte slurry is sprayed on the battery pole piece containing the polymer electrolyte layer, and the spraying distance is set to 200 mm, the spraying angle is 90°, the nozzle diameter is 2.0 mm, the high-pressure pump pressure is 15 MPa, the atomization pressure is set to 0.5 MPa, the spraying flow rate is controlled at 200 mL / min, and the spray width is 300 mm, forming a second solid electrolyte layer with a thickness of 15 μm on the composite pole piece;
[0222] (7) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0223] Example 2
[0224] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0225] (1) Boron nitride, carbon nanotubes, and polyvinylidene fluoride were mixed uniformly in a ball mill at a mass ratio of 8:1:1, with a rotation speed of 200 r / min and a grinding time of 3 hours. The mixture was added to a DMF solvent to prepare a slurry with a solid content of 40% by mass, and the mixture was fully stirred for 6 hours;
[0226] (2) spraying the slurry onto the surface of the lithium iron phosphate positive electrode plate by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 25 MPa, the atomization pressure to 0.3 MPa, the spraying flow rate to 100 mL / min, and the spray width to 300 mm, to obtain an interface modification layer containing an interface modification material with a thickness of 5 μm;
[0227] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0228] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the lithium iron phosphate positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0229] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0230] (5) Li 7 La 3 Zr 2 O 12 The solid electrolyte was dissolved in DMF solvent, stirred thoroughly and added with dispersant. After sand milling for 2 hours, the obtained solution was 7 La 3 Zr 2 O 12, polyvinylidene fluoride, and polypentylene succinate in a mass ratio of 23:1:1, adding polyvinylidene fluoride and polypentylene succinate to prepare a slurry with a solid content of 60% by mass;
[0231] (6) Use high-pressure atomization spray to coat Li 7 La 3 Zr 2 O 12 The solid electrolyte slurry is sprayed on the battery pole piece containing the polymer electrolyte layer, and the spraying distance is set to 200 mm, the spraying angle is 90°, the nozzle diameter is 2.0 mm, the high-pressure pump pressure is 15 MPa, the atomization pressure is set to 0.5 MPa, the spraying flow rate is controlled at 200 mL / min, and the spray width is 300 mm, forming a second solid electrolyte layer with a thickness of 15 μm on the composite pole piece;
[0232] (7) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0233] Example 3
[0234] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0235] (1) Magnesium oxide, carbon nanotubes, and polyvinylidene fluoride-hexafluoropropylene are mixed in a mass ratio of 8:
[0236] 1:1, mix evenly in a ball mill, set the speed to 200r / min, the duration of 3 hours, add the mixture into DMF solvent to prepare a slurry with a solid content of 40% by mass, and stir thoroughly for 6 hours;
[0237] (2) spraying the slurry onto the surface of the lithium iron phosphate positive electrode plate by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 25 MPa, the atomization pressure to 0.3 MPa, the spraying flow rate to 100 mL / min, and the spray width to 300 mm, to obtain an interface modification layer containing an interface modification material with a thickness of 5 μm;
[0238] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0239] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the lithium iron phosphate positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0240] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0241] (5) dissolving tantalum-doped lithium lanthanum zirconium oxide solid electrolyte in DMF solvent, stirring thoroughly and adding dispersant, and after sand milling the obtained solution for 2 hours, adding polyvinylidene fluoride and polypentylene succinate according to the mass ratio of tantalum-doped lithium lanthanum zirconium oxide, polyvinylidene fluoride and polypentylene succinate of 23:1:1 to prepare a slurry with a solid content of 60% by mass;
[0242] (6) spraying tantalum-doped lithium lanthanum zirconium oxide solid electrolyte slurry on the battery electrode containing the polymer electrolyte layer by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 15 MPa, the atomization pressure to 0.5 MPa, the spraying flow rate to 200 mL / min, and the spray width to 300 mm, to form a second solid electrolyte layer with a thickness of 15 μm on the composite electrode;
[0243] (7) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0244] Example 4
[0245] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0246] (1) Magnesium oxide, carbon nanotubes, and polyvinylidene fluoride-hexafluoropropylene are mixed in a mass ratio of 8:
[0247] 1:1, mix evenly in a ball mill, set the speed to 200r / min, the duration of 3 hours, add the mixture into DMF solvent to prepare a slurry with a solid content of 40% by mass, and stir thoroughly for 6 hours;
[0248] (2) The slurry was sprayed on the surface of the lithium cobalt oxide positive electrode sheet by high-pressure atomization spraying, with the spraying distance set to 200 mm, the spraying angle set to 90°, the nozzle diameter set to 2.0 mm, the high-pressure pump pressure set to 25 MPa, the atomization pressure set to 0.3 MPa, and the spraying flow rate set to 100
[0249] mL / min, spray width 300mm, to obtain an interface modification layer containing the interface modification material with a thickness of 5 μm;
[0250] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0251] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the lithium cobalt oxide positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0252] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0253] (5) dissolving tantalum-doped lithium lanthanum zirconium oxide solid electrolyte in DMF solvent, stirring thoroughly and adding dispersant, and after sand milling the obtained solution for 2 hours, adding polyvinylidene fluoride and polypentylene succinate according to the mass ratio of tantalum-doped lithium lanthanum zirconium oxide, polyvinylidene fluoride and polypentylene succinate of 23:1:1 to prepare a slurry with a solid content of 60% by mass;
[0254] (6) spraying tantalum-doped lithium lanthanum zirconium oxide solid electrolyte slurry on the battery electrode containing the polymer electrolyte layer by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 15 MPa, the atomization pressure to 0.5 MPa, the spraying flow rate to 200 mL / min, and the spray width to 300 mm, to form a second solid electrolyte layer with a thickness of 15 μm on the composite electrode;
[0255] (7) hot pressing the composite electrode to integrate, wherein the hot pressing temperature is 50° C., the pressure is 0.3 MPa, and the hot pressing time is 10 minutes;
[0256] (8) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0257] Example 5
[0258] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0259] (1) Aluminum nitride, conductive carbon black, and polyvinylidene fluoride were mixed uniformly in a ball mill at a mass ratio of 8:1:1, and the speed was set at 200 r / min for 3 hours. The mixture was added to DMF solvent to prepare a slurry with a solid content of 40% by mass, and the mixture was fully stirred for 6 hours;
[0260] (2) spraying the slurry on the surface of the NCM622 positive electrode sheet by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 25 MPa, the atomization pressure to 0.3 MPa, the spraying flow rate to 100 mL / min, and the spray width to 300 mm, to obtain an interface modification layer containing an interface modification material with a thickness of 5 μm;
[0261] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0262] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the NCM622 positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0263] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0264] (5) Li 7 La 3 Zr 2 O 12 The solid electrolyte was dissolved in DMF solvent, stirred thoroughly and added with dispersant. After sand milling for 2 hours, the obtained solution was 7 La 3 Zr 2 O 12 , polyvinylidene fluoride, and polypentylene succinate in a mass ratio of 23:1:1, adding polyvinylidene fluoride and polypentylene succinate to prepare a slurry with a solid content of 60% by mass;
[0265] (6) Use high-pressure atomization spray to coat Li 7 La 3 Zr 2 O 12 The solid electrolyte slurry is sprayed on the battery pole piece containing the polymer electrolyte layer, and the spraying distance is set to 200 mm, the spraying angle is 90°, the nozzle diameter is 2.0 mm, the high-pressure pump pressure is 15 MPa, the atomization pressure is set to 0.5 MPa, the spraying flow rate is controlled at 200 mL / min, and the spray width is 300 mm, forming a second solid electrolyte layer with a thickness of 15 μm on the composite pole piece;
[0266] (7) hot pressing the composite electrode to integrate, wherein the hot pressing temperature is 50° C., the pressure is 0.3 MPa, and the hot pressing time is 10 minutes;
[0267] (8) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0268] Example 6
[0269] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0270] (1) Aluminum nitride, conductive carbon black, and polyvinylidene fluoride were mixed uniformly in a ball mill at a mass ratio of 8:1:1, and the speed was set at 200 r / min for 3 hours. The mixture was added to DMF solvent to prepare a slurry with a solid content of 40% by mass, and the mixture was fully stirred for 6 hours;
[0271] (2) spraying the slurry on the surface of the NCM622 positive electrode sheet by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 25 MPa, the atomization pressure to 0.3 MPa, the spraying flow rate to 100 mL / min, and the spray width to 300 mm, to obtain an interface modification layer containing an interface modification material with a thickness of 5 μm;
[0272] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0273] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the NCM622 positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0274] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0275] (5) Li 7 La 3 Zr 2 O 12 Solid electrolyte, PVDF-HFP, and LiTFSI were dissolved in DMF solvent in a mass ratio of 2:5:3, stirred thoroughly, and a dispersant was added to prepare a composite solid electrolyte slurry with a solid content of 60 mass % and sand-milled for 1 hour;
[0276] (6) Spraying the composite solid electrolyte slurry on the battery electrode containing the polymer electrolyte layer by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 15 MPa, the atomization pressure to 0.5 MPa, the spraying flow rate to 200 mL / min, and the spray width to 300 mm, to form a second solid electrolyte layer with a thickness of 20 μm on the composite electrode;
[0277] (7) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0278] Example 7
[0279] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0280] (1) Aluminum nitride, conductive carbon black, and polyvinylidene fluoride were mixed uniformly in a ball mill at a mass ratio of 8:1:1, and the speed was set at 200 r / min for 3 hours. The mixture was added to DMF solvent to prepare a slurry with a solid content of 40% by mass, and the mixture was fully stirred for 6 hours;
[0281] (2) spraying the slurry onto the surface of the lithium iron phosphate positive electrode plate by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 25 MPa, the atomization pressure to 0.3 MPa, the spraying flow rate to 100 mL / min, and the spray width to 300 mm, to obtain an interface modification layer containing an interface modification material with a thickness of 5 μm;
[0282] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0283] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the lithium iron phosphate positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0284] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0285] (5) Tantalum-doped lithium lanthanum zirconium oxide solid electrolyte, PVDF-HFP, and LiTFSI were mixed in a mass ratio of 2:5:
[0286] 3. Dissolve in DMF solvent, stir thoroughly and add dispersant to prepare composite solid electrolyte slurry with solid content of 60 mass % and sand grind for 1 hour;
[0287] (6) Spraying the composite solid electrolyte slurry on the battery electrode containing the polymer electrolyte layer by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 15 MPa, the atomization pressure to 0.5 MPa, the spraying flow rate to 200 mL / min, and the spray width to 300 mm, to form a second solid electrolyte layer with a thickness of 20 μm on the composite electrode;
[0288] (7) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0289] Example 8
[0290] The present invention provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, wherein a multi-layer composite pole piece is prepared by high-pressure atomization spraying, and the specific steps are as follows:
[0291] (1) Aluminum nitride, styrene-butadiene rubber, sodium hydroxymethyl cellulose, and carbon nanotubes were mixed uniformly in a ball mill at a mass ratio of 7:1:1:1, and the speed was set at 200 r / min for 3 hours. The mixture was added into deionized water to prepare a slurry with a solid content of 60% by mass, and the mixture was fully stirred for 3 hours;
[0292] (2) spraying the slurry onto the surface of the lithium iron phosphate positive electrode sheet by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 89°, the nozzle diameter to 3.0 mm, the high-pressure pump pressure to 25 MPa, the atomization pressure to 0.3 MPa, the spraying flow rate to 100 mL / min, and the spray width to 300 mm, to obtain an interface modification layer containing an interface modification material with a thickness of 5 μm;
[0293] (3) PVDF-HFP, polypentane succinate and LiTFSI were sequentially added into DMF solvent in a mass ratio of 6:1:3, stirred at 65° C. for 8 h to mix evenly, and a dispersant was added to obtain a slurry with a solid content of 45% by mass;
[0294] (4) In a dry environment with a moisture content of less than 1 ppm, the polymer solid electrolyte slurry was sprayed on the lithium iron phosphate positive electrode sheet containing the interface modification layer by high-pressure atomization spraying. The spraying distance was set to 200 mm, the spraying angle was 90°, the nozzle diameter was 2.0 mm, the high-pressure pump pressure was 25 MPa, the atomization pressure was set to 0.4 MPa, and the spraying flow rate was controlled at 100
[0295] mL / min, spray width 300mm, forming a flexible polymer solid electrolyte layer with a thickness of 15μm on the composite electrode;
[0296] (5) Tantalum-doped lithium lanthanum zirconium oxide solid electrolyte, PVDF-HFP, and LiTFSI were mixed in a mass ratio of 2:5:
[0297] 3. Dissolve in DMF solvent, stir thoroughly and add dispersant to prepare composite solid electrolyte slurry with solid content of 60 mass % and sand grind for 1 hour;
[0298] (6) Spraying the composite solid electrolyte slurry on the battery electrode containing the polymer electrolyte layer by high-pressure atomization spraying, setting the spraying distance to 200 mm, the spraying angle to 90°, the nozzle diameter to 2.0 mm, the high-pressure pump pressure to 15 MPa, the atomization pressure to 0.5 MPa, the spraying flow rate to 200 mL / min, and the spray width to 300 mm, to form a second solid electrolyte layer with a thickness of 20 μm on the composite electrode;
[0299] (7) The multilayer composite solid-state battery pole piece and the lithium metal negative electrode obtained in the above steps are stacked and packaged, and then hot-pressed to obtain a solid-state battery, wherein the hot-pressing temperature is 60° C., the pressure is 0.5 MPa, and the hot-pressing time is 30 minutes.
[0300] Example 9
[0301] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that no inorganic / organic composite solid electrolyte layer is provided on the flexible polymer solid electrolyte layer.
[0302] Example 10
[0303] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that the total thickness of the solid electrolyte layer on the composite electrode sheet is 80 μm, and the total thickness of the three layers is not within the range of 5-50 μm.
[0304] Embodiment 11
[0305] This embodiment provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite pole piece. The difference from Example 1 is that the thickness of the interface modification layer on the composite pole piece is 55 μm, and the thickness of the interface modification material is not in the range of 500 nm to 10 μm.
[0306] Example 12
[0307] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that the applied high-pressure pump pressure is 35 MPa, which is not within the range of 10 to 30 MPa, and the high-pressure pump pressure is greater than the upper limit.
[0308] Embodiment 13
[0309] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that the applied high-pressure pump pressure is 5MPa, and the high-pressure pump pressure is less than the lower limit.
[0310] Embodiment 14
[0311] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that the spray width used is 500 mm, which is higher than the upper limit of the spray width.
[0312] Embodiment 15
[0313] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that the applied atomization pressure is greater than the upper limit, which is 1.2 MPa.
[0314] Example 16
[0315] This embodiment provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that the applied atomization pressure is less than the lower limit, which is 0.15 MPa.
[0316] Comparative Example 1
[0317] This comparative example provides a method for preparing an electrode sheet with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite electrode sheet. The difference from Example 1 is that an interface modification layer containing an interface modification material is not provided.
[0318] Comparative Example 2
[0319] This comparative example provides a method for preparing a pole piece with a multi-layer solid electrolyte and a solid-state battery, and uses high-pressure atomization spraying to prepare a multi-layer composite pole piece. The difference from Example 1 is that a flexible polymer solid electrolyte layer is not provided.
[0320] Performance Test:
[0321] Peel strength test: It is carried out in a peel force tester. At room temperature of 25°C and air humidity of -40°C dew point environment, one side of the prepared battery electrode collector is adhered to the working panel with a test double-sided tape, and the active material surface and the peel force tester are connected with a test tape. The peeling speed is 60mm / min and the peeling angle is 180°. The peeling force is tested and recorded.
[0322] Interface impedance test: The prepared composite electrode and lithium metal sheet were assembled into a button cell, and the AC impedance was tested in an electrochemical workstation using the AC impedance method. The voltage amplitude was set to 5 mV and the frequency range was 0.1 Hz to 1 MHz for testing.
[0323] Cycle stability test: The positive electrode sheet and the negative electrode sheet, the positive electrode sheet containing a solid electrolyte or the negative electrode sheet are cut and assembled into button batteries, and charged and discharged at a rate of 0.2C at 25°C. Each embodiment is cycled 200 times, and the battery capacity before and after the cycle is recorded 200 times, and the first charge and discharge capacity is recorded, and the first coulombic efficiency is calculated.
[0324] Table 1
[0325]
[0326]
[0327] By analyzing and comparing the test data in Table 1, the test results of Examples 1-16 and Comparative Examples 1-2 show that when preparing a multilayer solid-state battery composite pole piece within the preferred range, the first solid electrolyte layer effectively increases the solid-solid contact area, the flexible polymer solid electrolyte optimizes the solid interface contact, and the introduction of the inorganic solid electrolyte or composite solid electrolyte layer further improves the battery's cycle stability and charge and discharge performance. After hot pressing integration, the formation of a partial filling layer reduces the interlayer interface impedance. The interface impedance in Example 1 is only 32.27Ω, which is significantly less than 193.67Ω in Comparative Example 1, and the battery pole piece has a higher peel strength. The improvement of the interlayer interface uses the same process method to avoid the agglomeration of active materials and increase the compatibility between layers. Under the premise of greatly improving production efficiency, the electrochemical performance of the solid-state battery is further optimized. In particular, in Examples 4 and 5, the composite pole piece is hot pressed and hot pressed integration is performed when preparing the solid-state battery, thereby further reducing the interlayer interface impedance. By comparing Example 1 with other examples and comparative examples, it can be seen that Comparative Example 2 without a flexible polymer solid electrolyte layer, Example 9 without an inorganic / organic composite solid electrolyte layer, Example 10 in which the three total thicknesses are not in the range of 5-50μm, Example 11 in which the thickness of the interface modification material is not in the range of 500nm~10μm, Example 12 and Example 13 in which the high-pressure pump pressure is not in the range of 10~30MPa, Example 14 in which the spray amplitude is higher than the upper limit, and Example 15 and Example 16 in which the atomization pressure is not in the range of 0.2~1.0MPa, all fail to reduce the interface impedance and fail to improve the electrochemical performance of the solid-state battery. Figure 1 This is the first charge and discharge curve of the multilayer solid-state battery electrode in Example 1. Its first charge and discharge efficiency is as high as 96.93%, and the cycle capacity retention rate at a rate of 0.2C reaches 97.61%.
[0328] Figure 2 This is a scanning electron microscope image of the multi-layer solid-state battery electrode prepared in Example 1. The solid electrolyte is evenly dispersed on the surface of the electrode to form a continuous and dense solid electrolyte layer.
[0329] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
[0330] Industrial Applicability
[0331] The present invention increases the interface contact between the solid electrolyte and the electrode active material, and between the solid electrolyte and the battery pole piece by making the solid-state battery pole piece contain a multilayer solid electrolyte such as an interface modification layer and an organic polymer solid electrolyte layer, so as to achieve the replacement of the diaphragm, build a stable solid-state battery interface, and improve the cycle stability of the solid-state battery. The present invention uses a high-pressure atomization spraying method to achieve the preparation of a solid-state battery pole piece with a multilayer solid electrolyte, and ensure the uniformity of the multilayer structure, prevent the agglomeration of tiny solute particles during the introduction of the slurry, and achieve uniform preparation of the battery pole piece containing a multilayer solid electrolyte, while accurately controlling the thickness of each solid electrolyte layer, thereby improving the energy density and safety of the solid-state battery.
Claims
1. A pole piece with a multi-layer solid electrolyte, characterized in that: The method comprises: an interface modification layer and an interface softening layer are sequentially arranged on a positive electrode sheet or a negative electrode sheet through electrode sheet compounding, The interface softening layer comprises an organic polymer solid electrolyte and a lithium salt, and the interface modification layer comprises an interface modification material; The interface modification layer can be partially filled into the interface softening layer and the electrode active material to form a filling layer containing the interface modification material and the solid electrolyte.
2. The pole piece according to claim 1, characterized in that: The pole piece with multi-layer solid electrolyte further includes a second solid electrolyte layer on the interface softening layer.
3. The pole piece according to claim 2, characterized in that: The total thickness of the interface modification layer, the interface softening layer and the second solid electrolyte layer is 5 μm to 50 μm.
4. The pole piece according to any one of claims 1 to 3, characterized in that: The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium difluorooxalatoborate; Preferably, in the interface softening layer, the mass ratio of the organic polymer solid electrolyte to the lithium salt is 2:1 to 8:
1.
5. The pole piece according to any one of claims 1 to 4, characterized in that: The second solid electrolyte layer also includes a composite solid electrolyte.
6. The pole piece according to claim 5, characterized in that: The mass ratio of the organic polymer solid electrolyte to the inorganic solid electrolyte in the second solid electrolyte layer is 93:7 to 7:
93.
7. The pole piece according to any one of claims 1 to 6, characterized in that: The interface modification material includes an inorganic ceramic material, and the inorganic ceramic material is selected from one or more of nitrides, carbides, metal oxides, non-metal oxides, and inorganic solid electrolytes; Preferably, the inorganic ceramic material is selected from one or more combinations of oxides, nitrides, borides, halides, carbides, dielectric ceramics, ferroelectric ceramics, piezoelectric ceramics, diatomaceous earth, mullite, montmorillonite and kaolin; The oxide includes one or more combinations of silicon oxide, boron oxide, magnesium oxide, copper oxide, nickel oxide, calcium oxide, aluminum oxide, titanium oxide, zirconium oxide, vanadium oxide, lanthanum oxide, beryllium oxide, yttrium oxide, cerium oxide, and lead zirconium titanate; Wherein, the nitride includes one or more combinations of silicon nitride, titanium nitride, aluminum nitride, boron nitride, magnesium nitride, zirconium nitride and silicon oxynitride; The carbide includes one or more of silicon carbide, boron carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, molybdenum carbide, manganese carbide, iron carbide, titanium carbide, and niobium carbide; Wherein, the dielectric ceramic, the ferroelectric ceramic, and the piezoelectric ceramic each include BaTiO3, MgTiO3, CaTiO3PbTiO3, SrTiO3, BaO·TiO2, BaO-Nd2O3-TiO2, LiNbO3, LiTaO3, Cd2Ta2O7, Pb2Nb2O7, Cd2Nb2O7, PbNb2O6, Sr 1-x Ba x Nb2O6、Ba2NaNb5O 15 One or more of .
8. The pole piece according to claim 2, characterized in that: The second solid electrolyte used for the second solid electrolyte layer is selected from one or more of an inorganic solid electrolyte, an organic polymer solid electrolyte, and a lithium salt.
9. The pole piece according to claim 5 or 8, characterized in that: The inorganic solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a borate solid electrolyte, a nitride solid electrolyte and a hydride solid electrolyte; Preferably, the organic polymer solid electrolyte is selected from one or more of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyacrylonitrile, polymethyl methacrylate, polypropylene carbonate, polyphenylene sulfide, polyethyl cyanoacrylate, polypentylene succinate, polyvinyl chloride, polyvinyl carbonate, polyvinyl pyrrolidone, chitosan, polyimide, polyacrylate, polyurethane, aramid, polyetherimide, polyamide, polysulfone, aromatic sulfone, polyaromatic sulfone, polyether sulfone, epoxy resin and polyphenylene sulfone resin.
10. The pole piece according to claim 9, characterized in that: The oxide solid electrolyte is selected from one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, a NASICON-type solid electrolyte and a LISICON-type solid electrolyte; The garnet-type solid electrolyte includes Li x LqCy y A z O 12 and / or Li x La 3-y B y Zr z O 12 ; Wherein, A is one or more of Ta, Nb, Mg, Ti, Te, and W, and B is one or more of Ca, Rb, Al, and Ga; The perovskite solid electrolyte includes Li 3.3 La 0.53 TiO3、Li 3x La 2 / 3-x TiO3 and Li x Sr y M z One or more of TaO3; wherein M is one or more of Zr and Nb; The NASICON-type solid electrolyte includes Li x Al y M z (PO4)3、Li x Y y Zr z (PO4)3, LiTi2(PO4)3, LiGe2(PO4)3 and LiGeTi(PO4)3; wherein M is one or more of Ti, Ge, Hf, Zn, Zr and Si; The LISICON type solid electrolyte includes Li 3+x (P 1-x Si x )O4 and / or Li 3+x Ge x V 1-x O4; The sulfide solid electrolyte is selected from Argyrodite solid electrolyte LiPSMX, Thio-LiSICON solid electrolyte Li 4-x A 1-x B x S4 and one or more of glassy sulfides; wherein M is one or more of O, Cu, Zn, Bi, Sn, Al, Mn, Ce and In, X is one or more of F, Cl, Br and I; A is one or more of Si, Sn, Ge and Zr, and B is one or more of O, P, Al, Zn and Ga; The glassy sulfide includes one or more of Li2S-P2S5, Li2S-GeS2, Li2S-SiS2, Li2S-SiS2-Li4SiO4, Li2S-B2S3, and Li2S-B2S3-LiI; The halide solid electrolyte includes LiX, Li2MX 4、 Li3M′X6、Li x M″ y Ln z Cl 3、 LiM″′Cl5X″ and Li 3- y Zr y M″″ 1-y Cl6; wherein X is one or more of F, Cl, Br, I, M is one or more of Mg, Mn, Fe, Zn and Cd, M' is one or more of O, In, Y, Yb, Sc, Ho, Er, M "is one or more of Ta, Zr, Ca and Al, Ln is one or more of La, Ce, Pr, Nd, Sm, M "' is selected from one or more of La, Ta, Nb, X "is selected from O, Cl, F or OH, M " " is selected from one or more of Y, Er, Yb, Ho, Lu; Among them, 0 <x<1,0<y<1,0<z<1; The borate solid electrolyte is selected from one or more of Li2B4O7, Li2O-B2O3-P2O5; The nitride solid electrolyte is selected from one or more of LiPON, Li3N, Li7PN4, and LiSi2N3; The hydride solid electrolyte includes but is not limited to one or more of Li3AlH6, LiBH4, LiNH2, Li2NH, LiBH4-LiNH2, LiBH4-LiX; wherein X is one or more of Cl, Br or I; Preferably, the perovskite-type oxide solid electrolyte is selected from lithium lanthanum titanium oxide; The garnet-type oxide solid electrolyte is selected from one or more of lithium lanthanum zirconium oxide, niobium-doped lithium lanthanum zirconium oxide, tantalum-doped lithium lanthanum zirconium oxide, and niobium-tantalum dual-doped lithium lanthanum zirconium oxide; The NASICON type oxide solid electrolyte is selected from one or more of lithium aluminum titanium phosphate, lithium yttrium titanium phosphate, and lithium aluminum germanium phosphate.
11. A method for preparing a pole piece with a multilayer solid electrolyte according to any one of claims 1 to 10, characterized in that: It includes the following steps: Step S2: spraying the slurry containing the interface modification material onto the surface of the positive electrode sheet or the negative electrode sheet by a high-pressure atomization spraying method to obtain a positive electrode sheet or a negative electrode sheet having an interface modification layer; Step S4: spraying the slurry containing the organic polymer solid electrolyte onto the interface modification layer obtained in step S2 by a high-pressure atomization spraying method to obtain a positive electrode sheet or a negative electrode sheet having the interface modification layer and the interface softening layer; and Optional step Sx: hot pressing the positive electrode sheet or the negative electrode sheet to partially fill the interface modification layer into the organic polymer solid electrolyte layer and the positive electrode sheet or the negative electrode sheet and form a filling layer containing the interface modification material and the organic polymer solid electrolyte.
12. The preparation method according to claim 11, characterized in that: The preparation method further comprises the following steps before step Sx: Step S6: Spraying the slurry containing the second solid electrolyte onto the organic polymer solid electrolyte layer obtained in step S4 by a high-pressure atomization spraying method, thereby obtaining a positive electrode sheet or a negative electrode sheet of a multilayer solid electrolyte having the interface modification layer, the interface softening layer containing the organic polymer solid electrolyte and the second solid electrolyte layer.
13. The preparation method according to claim 12, characterized in that: The solid contents of the slurry containing the interface modification material, the slurry containing the organic polymer solid electrolyte and the slurry containing the second solid electrolyte are 5-80% by mass, preferably 10-60% by mass, respectively.
14. The preparation method according to claim 12, characterized in that: In the high-pressure atomization spraying method in step S2, step S4 and step S6, the spraying conditions are as follows: the pressure of the high-pressure pump is 10-30 MPa, the diameter of the nozzle is 0.5-3.0 mm, the spray width is 50-400 mm, the atomization pressure is 0.2-1.0 MPa, the spray flow rate is 50-450 mL / min, the spray distance is 20-350 mm, and the spray angle is 80-93°; Preferably, the spraying conditions in step S2, step S4 and step S6 are the same or different.
15. The preparation method according to any one of claims 11 to 14, characterized in that: The slurry in step S2 further comprises one or more of a conductive agent and a binder; Preferably, the slurry in step S4 further comprises an inorganic solid electrolyte; Preferably, the slurry in step S4 and the slurry in step S6 each further comprise a binder; Preferably, when the second solid electrolyte in step S6 includes only an organic polymer solid electrolyte, the slurry in step S6 includes a lithium salt.
16. The preparation method according to claim 15, characterized in that: The conductive agent is selected from one or more of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, graphene, carbon nanofibers, carbon molecular sieves, polyethylene dioxythiophene, polystyrene sulfonic acid and lithium polystyrene sulfonate; Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium difluorooxalatoborate; Preferably, the binder is selected from one or more of polyvinylidene fluoride, polyvinyl alcohol, polytetrafluoroethylene, sodium hydroxymethyl cellulose, styrene-butadiene rubber, nitrile rubber, styrene-butadiene-styrene copolymer, polyacrylic acid, and lithium polyacrylate; Preferably, the binder contained in the slurry in step S2, the slurry in step S2 and the slurry in step S6 are the same as or different from each other; Preferably, the slurry in step S4 and the lithium salt contained in the slurry in step S4 are the same or different.
17. The preparation method according to any one of claims 11 to 16, characterized in that: In the hot pressing of step Sx, the hot pressing temperature is 40 to 60° C., the pressure is 0.1 to 0.5 MPa, and the hot pressing time is 5 to 20 minutes.
18. A solid-state battery, characterized in that: A pole piece comprising the pole piece described in any one of claims 1 to 10 or a pole piece obtained by the preparation method described in any one of claims 11 to 17.
19. A method for preparing a solid-state battery, characterized in that: include: A step of preparing a positive electrode sheet and / or a negative electrode sheet having a multilayer solid electrolyte by the preparation method according to any one of claims 11 to 17; The positive electrode sheet and the negative electrode sheet are stacked and packaged, and then hot-pressed to integrate them.
20. The preparation method according to claim 19, characterized in that: In the hot pressing integration, the hot pressing temperature is 50 to 80° C., the pressure is 0.2 to 0.8 MPa, and the hot pressing time is 20 to 40 minutes.
Citation Information
Cited By
Lithium-loving elastic electrolyte, preparation method thereof and solid-state lithium metal battery
CN120127213A
Composite solid electrolyte layer and preparation method and application thereof