Secondary battery and electric equipment

By using a variety of conductive materials and specific ratio binders in the negative electrode sheet of the secondary battery, the problem of poor fast charging performance of the secondary battery is solved, and the charging rate and dynamic performance are significantly improved.

CN119008853AActive Publication Date: 2024-11-22SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411018285.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-22
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The fast charging performance of existing secondary batteries is poor and cannot meet the high requirements for rapid discharge performance of electric vehicles.

Method used

A secondary battery is designed, and its negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer arranged on the negative electrode current collector. The negative electrode active material layer is composed of a negative electrode active material, a conductive agent and a binder, and the conductive agent is at least composed of The two different conductive materials are composed of, satisfying the specific tap density and molar mass ratio relationship, and constructing a conductive network of electrodes to improve ion and electron conductivity.

Benefits of technology

It effectively improves the fast charging performance of the secondary battery and achieves excellent charging rate performance and dynamic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention provides a secondary battery and electric equipment, the secondary battery provided by the invention comprises a negative pole piece, a conductive agent in the negative pole piece is composed of at least two different conductive materials, and the secondary battery satisfies: 10lt; [100000 * (Dv50)] / [P2 * (lnM)] lt; 34; wherein P g / L is the tap density of the conductive agent; dv50 [mu] m is the corresponding particle size when the volume cumulative distribution percentage of the negative electrode active material is equal to 50%; m g / mol is the molar mass of the binder. The conductive agent is composed of at least two different conductive materials and is matched with the relationship among the Dv50 of the negative electrode active material, the tap density of the conductive agent and the molar mass of the binder, so that a pole piece conductive network is effectively constructed, the ionic conductivity and the electronic conductivity of the negative pole piece are improved, and the charging rate performance is effectively improved; and the secondary battery with excellent rapid charging performance is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery manufacturing, in particular to a secondary battery and electrical equipment. Background Art

[0002] At present, the negative electrode is an important component of secondary batteries, and its kinetic performance is a key factor affecting the performance of secondary batteries.

[0003] In the prior art, electric vehicles have put forward higher requirements on the rapid discharge performance of secondary batteries. However, the rapid discharge performance of existing secondary batteries is poor and cannot effectively meet the demand for excellent rapid charging of secondary batteries.

[0004] Therefore, there is an urgent need to provide a negative electrode plate with excellent kinetic performance to improve the fast charging performance of secondary batteries. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a secondary battery and an electrical device to solve the problem that the existing secondary battery has poor fast charging performance.

[0006] In order to solve the above problems, the present invention is achieved through the following technical solutions:

[0007] The present invention provides a secondary battery, which includes a negative electrode plate, wherein the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder; the conductive agent is composed of at least two different conductive materials;

[0008] The secondary battery satisfies: 10<[100000*(Dv50)] / [P 2 *(lnM)]<34;

[0009] Wherein, P g / L is the tap density of the conductive agent;

[0010] Dv50μm is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material is equal to 50%;

[0011] M g / mol is the molar mass of the binder.

[0012] Furthermore, in the secondary battery, the conductive agent includes at least two of a zero-dimensional point conductive agent, a one-dimensional line conductive agent, and a two-dimensional surface conductive agent.

[0013] Furthermore, in the secondary battery, the conductive agent includes a zero-dimensional point conductive agent, a one-dimensional line conductive agent and a two-dimensional surface conductive agent.

[0014] Furthermore, based on the total content of the conductive agent, the mass percentage of the zero-dimensional point conductive agent is 25-40%, the mass percentage of the one-dimensional line conductive agent is 30-50%, and the mass percentage of the two-dimensional planar conductive agent is 10-45%.

[0015] Furthermore, in the secondary battery, among the conductive agents, the zero-dimensional point-shaped conductive agent includes at least conductive carbon black, the one-dimensional linear conductive agent includes at least one of carbon nanotubes and carbon fibers, and the two-dimensional planar conductive agent includes at least graphene.

[0016] Furthermore, in the secondary battery, the tap density P of the conductive agent is 120-210, the Dv50 of the negative electrode active material is 40-100, and the molar mass M of the binder is 1200000-1900000.

[0017] Furthermore, the secondary battery meets at least one of the following conditions:

[0018] a. The Dv50 of the zero-dimensional point-shaped conductive agent is 30 to 100 μm, the Dv50 of the one-dimensional line-shaped conductive agent is 4 to 20 μm, and the Dv50 of the two-dimensional planar conductive agent is 0.5 to 3 μm;

[0019] b. The binder is one or more of styrene-butadiene latex, polytetrafluoroethylene, and PVDF.

[0020] Furthermore, in the secondary battery, the negative electrode active material has a pore structure, and the ratio K of open pores to closed pores of the negative electrode active material is 2-3.

[0021] Furthermore, in the secondary battery, the negative electrode active material includes secondary particles formed by aggregation of primary particles, and the number N of primary particles in a single secondary particle is 40 to 60.

[0022] The present invention further provides an electric device, which includes the above-mentioned secondary battery, and the secondary battery serves as a power supply for the electric device.

[0023] Compared with the prior art, the embodiments of the present invention have the following advantages:

[0024] In an embodiment of the present invention, a secondary battery is provided, which includes a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder; the conductive agent is composed of at least two different conductive materials; the secondary battery satisfies: 10<[100000*(Dv50)] / [P 2*(lnM)]<34; wherein, P g / L is the tap density of the conductive agent; Dv50μm is the particle size corresponding to the cumulative volume distribution percentage of the negative electrode active material being equal to 50%; M g / mol is the molar mass of the binder. In the embodiment of the present invention, by setting the conductive agent to be composed of at least two different conductive materials, and matching the Dv50 of the negative electrode active material, the tap density of the conductive agent powder and the molar mass of the binder to satisfy the above relationship, an effective electrode conductive network is constructed, the ionic conductivity and electronic conductivity of the negative electrode electrode are improved, thereby effectively improving the charge rate performance.

[0025] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. DETAILED DESCRIPTION

[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.

[0027] The applicant of the present invention has found that during the charging process of a sodium ion battery, sodium ions are deintercalated from the positive electrode and intercalated into the negative electrode through the electrolyte. Therefore, the kinetic performance of the negative electrode sheet of the sodium ion battery is closely related to the fast charging performance of the battery. However, the fast charging performance of existing secondary batteries such as sodium ion batteries is poor.

[0028] In order to solve the above problems, an embodiment of the present invention provides a secondary battery, which includes a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder; the conductive agent is composed of at least two different conductive materials;

[0029] The secondary battery satisfies: 10<[100000*(Dv50)] / [P 2 *(lnM)]<34;

[0030] Wherein, Pg / L is the tap density of the conductive agent;

[0031] Dv50μm is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material is equal to 50%;

[0032] M g / mol is the molar mass of the binder.

[0033] The applicant found that the kinetic performance of the negative electrode plate depends on the mutual matching of the physicochemical properties between the various components of the negative electrode; at the same time, the kinetic performance of the negative electrode plate is closely related to the fast charging performance of the battery. Therefore, by optimizing the physicochemical properties between the various components of the negative electrode plate and making reasonable matches, the kinetic performance of the negative electrode plate can be effectively improved, thereby improving the fast charging performance of the battery.

[0034] Because the three parameters of the negative electrode active material's Dv50, the tap density of the conductive agent powder and the molar mass of the binder play a decisive role in the negative electrode dynamics, in the embodiment of the present invention, based on the interaction and mutual influence relationship between the negative electrode active material, the conductive agent powder and the binder, the conductive agent is arranged to be composed of at least two different conductive materials, and the Dv50 of the negative electrode active material, the tap density of the conductive agent powder and the molar mass of the binder are matched to satisfy the above relationship, so as to effectively construct a conductive network of the electrode sheet, improve the ionic conductivity and electronic conductivity of the negative electrode sheet, thereby effectively improving the charging rate performance, and preparing a secondary battery with excellent fast charging performance.

[0035] Alternatively, [100000*(Dv50)] / [P 2 The value of [(lnM)] can be a range of one or any two of 11, 15, 20, 30, 33.

[0036] Optionally, in one embodiment, the above-mentioned conductive agent includes at least two of a zero-dimensional point conductive agent, a one-dimensional linear conductive agent, and a two-dimensional surface conductive agent. Under the joint action of at least two conductive agents of different dimensions, a three-dimensional conductive network can be constructed, thereby greatly improving the dynamic performance of the battery.

[0037] Optionally, in a specific embodiment, in the secondary battery provided by the embodiment of the present invention, the specific surface area of ​​the zero-dimensional point-shaped conductive agent is 30 to 200 m 2 / g, the specific surface area of ​​the one-dimensional linear conductive agent is 300 to 1000 m 2 / g, the specific surface area of ​​the two-dimensional planar conductive agent is 2000~3000m 2 In some embodiments, the specific surface area of ​​the zero-dimensional point-shaped conductive agent is 30 m 2 / g, 35m 2 / g, 40m 2 / g, 60m 2 / g, 80m 2 / g、100m 2 / g, 150m 2 / g, 200m 2 / g or any two of them, the specific surface area of ​​the one-dimensional linear conductive agent is 300m 2 / g, 350m2 / g, 400m 2 / g、500m 2 / g、700m 2 / g、900m 2 / g、1000m 2 / g or any two of them, the specific surface area of ​​the two-dimensional planar conductive agent is 2000m 2 / g, 2100m 2 / g, 2200m 2 / g, 2400m 2 / g, 2500m 2 / g, 2600m 2 / g、2800m 2 / g、3000m 2 / g or both.

[0038] Optionally, in a specific embodiment, in the secondary battery provided by the embodiment of the present invention, the Dv50 of the zero-dimensional point-shaped conductive agent is 30 to 100 μm, the Dv50 of the one-dimensional linear conductive agent is 4 to 20 μm, and the Dv50 of the two-dimensional planar conductive agent is 0.5 to 3 μm; in some embodiments, the Dv50 of the zero-dimensional point-shaped conductive agent can be in the range of 30 μm, 40 μm, 50 μm, 60 μm, 80 μm, 100 μm, or any two of them. The Dv50 of a one-dimensional linear conductive agent can be in the range of 4μm, 5μm, 8μm, 10μm, 15μm, 20μm or any two of them; the Dv50 of a two-dimensional planar conductive agent can be in the range of 0.5μm, 0.6μm, 0.8μm, 1μm, 1.5μm, 2μm, 3μm or any two of them, so that the size of the conductive agent in each dimension is moderate, which can give full play to the performance advantages of the conductive agent in each dimension and improve the fast charging performance.

[0039] Optionally, in a specific embodiment, in the secondary battery provided by the embodiment of the present invention, the tap density of the zero-dimensional point-shaped conductive agent is 200-500 g / L, the tap density of the one-dimensional linear conductive agent is 100-250 g / L, and the tap density of the two-dimensional surface conductive agent is 10-100 g / L, which can effectively take into account the wetting effect with the electrolyte and the contact performance with the negative electrode active material, form a dense conductive network, have high ionic conductivity, and achieve excellent fast charging performance. In some embodiments, the tap density of the zero-dimensional point conductive agent is in the range of 200 g / L, 250 g / L, 350 g / L, 500 g / L or any two of the range values, the tap density of the one-dimensional linear conductive agent is in the range of 100 / L, 120 g / L, 150 g / L, 160 g / L, 180 g / L, 200 g / L, 220 g / L, 250 g / L or any two of the range values, and the tap density of the two-dimensional planar conductive agent is in the range of 10 g / L, 20 g / L, 40 g / L, 60 g / L, 80 g / L, 100 g / L or any two of the range values.

[0040] In practical applications, the test method for tap density is determined by the tap density measurement method in GB / T 31057.2-2018. The specific steps include:

[0041] Put the weighed powder into the measuring cylinder of the vibration compaction device, and fix the measuring cylinder on the support; rotate the cam, and the directional rod drives the support to slide up and down and hit the anvil; vibrate 250±15 times per minute for 12 minutes; measure the volume of the powder in the measuring cylinder, and the ratio of the powder mass to the volume is the tap density of the powder.

[0042] Optionally, in one embodiment, the conductive agent in the above-mentioned secondary battery includes a zero-dimensional point conductive agent, a one-dimensional linear conductive agent and a two-dimensional surface conductive agent, and based on the total content of the conductive agent, the mass percentage of the zero-dimensional point conductive agent is 25-40%, the mass percentage of the one-dimensional linear conductive agent is 30-50%, and the mass percentage of the two-dimensional surface conductive agent is 10-45%. In this way, a three-dimensional conductive network is more reasonably constructed to achieve fast charging performance.

[0043] Optionally, in one embodiment, the zero-dimensional point-shaped conductive agent includes at least conductive carbon black, the one-dimensional linear conductive agent includes at least one of carbon nanotubes and carbon fibers, and the two-dimensional planar conductive agent includes at least graphene.

[0044] Optionally, in one embodiment, the tap density P g / L of the conductive agent is 120 to 210 g / L, and the tap density P of the conductive agent is the tap density of a mixed conductive agent obtained by mixing at least two of a zero-dimensional point conductive agent, a one-dimensional linear conductive agent, and a two-dimensional surface conductive agent. The tap density of the conductive agent within the above range can effectively take into account both the wetting effect with the electrolyte and the contact performance with the negative electrode active material, thereby forming a dense conductive network with high ionic conductivity and achieving excellent rapid discharge performance.

[0045] In one embodiment, the Dv50 of the negative electrode active material is 40 to 100 μm, so that the particle size is moderate, which not only facilitates the rapid shuttle of active ions between particles to achieve rapid charging, but also avoids excessive liquid absorption during the stirring process and too low solid content of the slurry, which leads to process problems such as coating cracks and bulging edges, thereby ensuring processing performance.

[0046] In one embodiment, the molar mass of the binder Mg / mol is 1200000 to 1900000 g / mol, which can ensure that the binder network layer formed on the surface of the negative electrode active material has a high porosity to avoid the rate performance being affected by too low liquid absorption; it can also avoid dispersion problems such as folding and agglomeration of the binder molecules, so that the negative electrode active material and the conductive agent can be evenly dispersed, thereby forming a good conductive network, which can effectively take into account both rate performance and rapid discharge performance.

[0047] In some embodiments, the tap density P g / L of the conductive agent may be 120 g / L, 110 g / L, 120 g / L, 140 g / L, 150 g / L, 160 g / L, 180 g / L, 200 g / L, 210 g / L, or any two of the range values, the Dv50 of the negative electrode active material may be 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm, or any two of the range values, and the molar mass of the binder may be 1,200,000 g / mol, 1,050,000 g / mol, 1,100,000 g / mol, 1,200,000 g / mol, 1,500,000 g / mol, 1,800,000 g / mol, or 1,900,000 g / mol, or any two of the range values.

[0048] Optionally, in a specific embodiment, the binder is one or more of styrene-butadiene latex, polytetrafluoroethylene, and PVDF.

[0049] Optionally, in one embodiment, the negative electrode active material has a porous structure, and the ratio K of the open pores to the closed pores of the negative electrode active material is 2 to 3, and the proportion of the open pores is moderate, so that the active surface area of ​​the material is moderate, and the first coulombic efficiency and rate performance can be effectively balanced to ensure the infiltration effect of the electrolyte. In some embodiments, the ratio K of the open pores to the closed pores of the negative electrode active material is 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, or any two of the range values.

[0050] In practical applications, the above K value can be obtained by adjusting the sintering temperature, the closed porosity can be obtained by GB / T 10707-2008 test, and the open porosity can be measured by gas adsorption method.

[0051] In the secondary battery provided by the embodiment of the present invention, the negative electrode active material includes secondary particles formed by aggregation of primary particles, and the number N of primary particles in a single secondary particle is 40 to 60, which can effectively take into account the first coulomb efficiency and rate performance, and can reduce the cycle gas production. Optionally, in some embodiments, the number N of primary particles in a single secondary particle can be 40, 42, 45, 48, 50, 52, 55, 58, 60, or any two of the range values.

[0052] In practical applications, the N value can be adjusted by the calcination time during the preparation of hard carbon. The N value can be measured by measuring the primary particle and secondary particle size and volume ratio by SEM and TEM.

[0053] Among them, the above-mentioned negative electrode active material layer can adopt negative electrode active materials used for batteries, for example, selected from metal negative electrode active materials or non-metallic negative electrode active materials; the metal negative electrode active material is preferably metal foil or alloy compound such as metallic sodium, sodium alloy, tin, antimony, etc.; the non-metallic negative electrode active material is preferably any one of hard carbon, soft carbon, graphite, silicon oxide, or a combination of at least two of them.

[0054] Optionally, in a specific embodiment, the negative electrode active material includes hard carbon, and the precursor of the hard carbon is one or more of biomass, resin, and coal, so that the crystal arrangement inside the negative electrode active material is disordered and the interlayer spacing is large, which is more conducive to the additives in the electrolyte forming a protective film on its surface, further optimizing the stability of the protective film. In this embodiment, the resin may include phenolic resin, epoxy resin, polyfurfuryl alcohol, etc.

[0055] Optionally, in a specific embodiment, the negative electrode current collector is one or more of copper foil, aluminum foil, carbon-coated copper foil, and carbon-coated aluminum foil.

[0056] In some embodiments, the negative electrode sheet is prepared as follows: the components for preparing the negative electrode sheet, such as the negative electrode active material, binder and conductive agent, are dispersed in a solvent such as deionized water to form a negative electrode slurry; the negative electrode slurry is coated on both sides of a negative electrode collector such as copper foil; after baking, rolling, cutting and other processes, the negative electrode sheet can be obtained.

[0057] The secondary battery provided by the present invention also includes a positive electrode plate and an electrolyte.

[0058] Among them, the electrolyte in the electrolyte plays the role of conducting ions between the positive electrode plate and the negative electrode plate.

[0059] The positive electrode plate includes a positive electrode current collector and a positive electrode active material layer arranged on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material. The positive electrode active material includes at least one of sodium ion transition metal oxides, sodium ion transition metal phosphates and variants, sodium ion transition metal sulfates, and Prussian blue compounds.

[0060] Optionally, in one embodiment, the positive electrode active material comprises NaCoO 2 、NaMnO 2 、NaNi 0.33 Fe 0.33 Mn 0.33 O 2 、NaFePO 4 、NaCoPO 4 、Na 3 V 2 (PO 4 ) 3 One or more of.

[0061] Optionally, in one embodiment, the positive electrode plate further includes an adhesive and a conductive agent, the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, and tetrafluoroethylene-hexafluoropropylene copolymer, and the conductive agent may be acetylene black, carbon fiber, carbon nanotubes, Ketjen black, artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, etc.

[0062] In some embodiments, the positive electrode sheet is prepared as follows: the components for preparing the positive electrode sheet, such as the positive electrode active material, the binder and any other components, are dispersed in a solvent such as N-methylpyrrolidone to form a positive electrode slurry; the positive electrode slurry is coated on both sides of a positive electrode collector such as aluminum foil; after baking, rolling, cutting and other processes, the positive electrode sheet can be obtained.

[0063] It can be understood that the secondary battery provided in the embodiment of the present invention further includes a separator.

[0064] In practical applications, the negative electrode sheet, the separator and the positive electrode sheet are stacked in order and wound to obtain a core, the core is packaged to obtain a bare cell, and the bare cell is baked and then injected, formed, sealed and sorted to obtain the above-mentioned secondary battery.

[0065] The present invention further provides an electric device, which includes the above-mentioned secondary battery, and the secondary battery serves as a power supply for the electric device.

[0066] For the above-mentioned secondary battery embodiment and electrical equipment embodiment, they include the above-mentioned electrolyte and can achieve the same technical effect. In order to avoid repetition, they will not be described here. For relevant details, please refer to the partial description of the positive electrode material embodiment.

[0067] In order to make the invention purpose, technical scheme and beneficial effect of the present invention clearer, the present invention is further described below in conjunction with embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0068] The present invention is described in detail below by way of examples.

[0069] (1) Charging rate performance test:

[0070] At room temperature, charge the cell with SOC = 0% to 4.0V at a current density of 0.33C, and record the capacity as C1.

[0071] Then, at room temperature, charge the cell with SOC=0% to 4.0V at a current density of 5C. The capacity at this time is C2, and the recorded capacity is C2.

[0072] The capacity retention ratio C2 / C1 is calculated as a test indicator of the charging rate performance.

[0073] (2) Coating crack test: Randomly cut 1 square decimeter of the baked negative electrode sheet and record the number of cracks on this area.

[0074] (3) Negative electrode ion conductivity test: The constant current intermittent titration method GITT test was used, with a voltage range of 2.5V to 4.2V, a pulse time of 10 minutes, a pulse current of 0.33C, and a relaxation time of 3 hours.

[0075] (4) Negative electrode electronic conductivity test: Electrode electronic conductivity = 1 / electrode membrane resistance. The membrane resistance is tested using the four-probe method. Using a four-probe instrument, place the probes in contact with the sample to be tested and measure its resistance.

[0076] (5) Negative electrode moisture absorption test: Take 1 square decimeter of negative electrode and place it in an environment with a humidity of 70% for 7 days. The increase in the mass of the electrode within 7 days is the moisture absorption.

[0077] (6) First Coulomb efficiency test:

[0078] The battery was discharged to 2.5V at 0.33C constant current, left standing for 30 minutes, charged to 4.2V at 0.33C constant current, and charged to 0.05C at constant voltage to obtain the first charge capacity of the battery. Left standing for 30 minutes, discharged to 2.5V at 0.33C constant current to obtain the first discharge capacity. First efficiency = first discharge capacity / first charge capacity*100%, calculate the first coulombic efficiency of the battery.

[0079] Example 1

[0080] (1) Preparation of positive electrode sheet

[0081] NaNi 0.33 Fe 0.33 Mn 0.33 O 2 , sodium carboxymethyl cellulose (CMC), conductive carbon black, and styrene-butadiene latex (SBR) are mixed in a mass ratio of 80:7.5:7.5:5, and solvent N-methylpyrrolidone is added, and the positive electrode slurry is obtained by stirring under the action of a vacuum mixer; the positive electrode slurry is evenly coated on both sides of the carbon-coated aluminum foil, and after drying at room temperature, it is transferred to an oven for further drying, and then rolled and cut into pieces to obtain the positive electrode sheet.

[0082] (2) Preparation of negative electrode sheet

[0083] Preparation of hard carbon: In an inert atmosphere, heat a phenolic resin with a molecular weight of about 1000g / mol to 1300℃ at 10℃ / min, calcine at high temperature for 12 hours, and then cool to room temperature to obtain hard carbon. According to a mass ratio of 97:1:2, mix hard carbon with a Dv50 of 6μm, a conductive agent with a tap density of 160g / L (a mixture of conductive carbon black, carbon nanotubes, and graphene in a mass ratio of 30:40:30) and styrene-butadiene latex (SBR) with a molar mass of 1500000g / mol, and evenly disperse them in deionized water to form a uniform black slurry. After coating the mixed slurry on both sides of the copper foil, it is baked, rolled, and cut into pieces to obtain the negative electrode sheet;

[0084] The hard carbon particle size Dv50 is 68 μm, the number of primary particles in a single secondary particle is 50, and the ratio of open pores to closed pores is 2.5;

[0085] The specific surface area of ​​conductive carbon black in the conductive agent is 100m 2 / g, Dv50 is 60μm, tap density is 260g / L, and the specific surface area of ​​carbon nanotubes is 600m2 / g, Dv50 is 10μm, tap density is 180g / L, and the specific surface area of ​​graphene is 2500m 2 / g, Dv50 is 2μm, and tap density is 60g / L.

[0086] (3) Preparation of electrolyte

[0087] Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1, and then 1 mol / L NaPF 6 Dissolve in a mixed organic solvent, mix evenly, and prepare an electrolyte.

[0088] (4) Preparation of batteries

[0089] The positive electrode sheet, the isolation film and the negative electrode sheet are stacked in sequence, then wound into a bare battery cell and loaded into a soft-pack shell. After top and side sealing, liquid injection, formation, sorting and other processes, a sodium ion battery is obtained.

[0090] Embodiments 2 to 4

[0091] The preparation method is the same as that of Example 1, except that, during the preparation of the negative electrode, the ratio of the conductive carbon black, the carbon nanotubes and the graphene is adjusted.

[0092] Embodiments 5 to 8

[0093] The preparation method is the same as that of Example 1, except that during the preparation of the negative electrode, the particle size Dv50 of the conductive carbon black, carbon nanotubes, and graphene is adjusted.

[0094] Among them, the particle sizes Dv50 of the conductive carbon black, carbon nanotubes, and graphene in Example 5 are 62 μm, 12 μm, and 3 μm, respectively;

[0095] The particle sizes Dv50 of the conductive carbon black, carbon nanotubes, and graphene in Example 6 are 65 μm, 14 μm, and 4 μm, respectively;

[0096] The particle sizes Dv50 of the conductive carbon black, carbon nanotubes, and graphene in Example 7 are 57 μm, 8 μm, and 1.5 μm, respectively;

[0097] The particle sizes Dv50 of the conductive carbon black, carbon nanotubes and graphene in Example 8 are 55 μm, 7 μm and 1 μm respectively.

[0098] Examples 9 to 12

[0099] The preparation method is the same as that of Example 1, except that, in the hard carbon preparation process, the particle size of the negative electrode material is changed by adjusting the molecular weight of the precursor phenolic resin. The larger the molecular weight, the larger the particle size.

[0100] Embodiments 13 to 16

[0101] The preparation method is the same as that of Example 1, except that the calcination time during the preparation of the hard carbon is adjusted to obtain negative electrode active materials with different N values. This is achieved by adjusting the calcination time of the hard carbon. The longer the time, the smaller the N value.

[0102] Examples 17 to 20

[0103] The preparation method is the same as that of Example 1, except that the calcination temperature during the preparation of the hard carbon is adjusted to obtain negative electrode active materials with different K values. The higher the temperature, the greater the K value.

[0104] Examples 21 to 23

[0105] The preparation method is the same as that of Example 1, except that binders with different molar masses are used as the binder for the negative electrode.

[0106] Embodiments 24 to 26

[0107] The preparation method is the same as that of Example 1, except that the components and proportions of the conductive agent are changed. As shown in Table 1.

[0108] Comparative Example 1-2

[0109] The preparation process is the same as that of Example 1, except that during the preparation of the negative electrode sheet, the mixing ratio of the conductive carbon black, carbon nanotubes and graphene is adjusted.

[0110] Comparative Example 3

[0111] The preparation process is the same as that of Example 1, except that, during the preparation of the negative electrode sheet, the conductive agent is only carbon nanotubes.

[0112] The process parameters of each embodiment and comparative example are shown in Table 1 and Table 2.

[0113] Table 1

[0114]

[0115]

[0116]

[0117] Where x = [100000*(Dv50)] / [P 2 *(lnM)].

[0118] The negative electrode sheets prepared in each embodiment and comparative example were subjected to ion conductivity test, electronic conductivity test and moisture absorption test, and the batteries prepared in each embodiment and comparative example were subjected to first coulomb efficiency test, charge rate performance test and coating crack test, wherein the test data are shown in Table 3.

[0119] Table 3

[0120]

[0121] In summary, in this embodiment, by setting the conductive agent to be composed of at least two different conductive materials, and matching the Dv50 of the negative electrode active material, the tap density of the conductive agent powder and the molar mass of the binder to satisfy the above relationship, an effective electrode conductive network is constructed, the ionic conductivity and electronic conductivity of the negative electrode are improved, thereby effectively improving the charging rate performance, and preparing a secondary battery with excellent fast charging performance.

[0122] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0123] The secondary battery and electrical equipment provided by the present invention are introduced in detail above. The principle and implementation mode of the present invention are explained by using specific examples in this article. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A secondary battery, characterized in that: The invention comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; wherein the conductive agent is composed of at least two different conductive materials; The secondary battery satisfies: 10<[100000*(Dv50)] / [P 2 *(lnM)]<34; Wherein, P g / L is the tap density of the conductive agent; Dv50μm is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material is equal to 50%; Mg / mol is the molar mass of the binder.

2. The secondary battery according to claim 1, characterized in that: The conductive agent includes at least two of a zero-dimensional point conductive agent, a one-dimensional line conductive agent, and a two-dimensional surface conductive agent.

3. The secondary battery according to claim 2, characterized in that: The conductive agent includes a zero-dimensional point conductive agent, a one-dimensional line conductive agent and a two-dimensional surface conductive agent.

4. The secondary battery according to claim 3, characterized in that: Based on the total content of the conductive agent, the mass percentage of the zero-dimensional point conductive agent is 25-40%, the mass percentage of the one-dimensional line conductive agent is 30-50%, and the mass percentage of the two-dimensional planar conductive agent is 10-45%.

5. The secondary battery according to any one of claims 2 to 4, characterized in that: Among the conductive agents, the zero-dimensional point-shaped conductive agent includes at least conductive carbon black, the one-dimensional line-shaped conductive agent includes at least one of carbon nanotubes and carbon fibers, and the two-dimensional planar conductive agent includes at least graphene.

6. The secondary battery according to claim 1, characterized in that: The tap density P of the conductive agent is 120-210, the Dv50 of the negative electrode active material is 40-100 μm, and the molar mass M of the binder is 1,200,000-1,900,000.

7. The secondary battery according to claim 2, characterized in that: Meet at least one of the following conditions: a. The Dv50 of the zero-dimensional point-shaped conductive agent is 30 to 100 μm, the Dv50 of the one-dimensional line-shaped conductive agent is 4 to 20 μm, and the Dv50 of the two-dimensional planar conductive agent is 0.5 to 3 μm; b. The binder is one or more of styrene-butadiene latex, polytetrafluoroethylene, and PVDF.

8. The secondary battery according to claim 1, characterized in that: The negative electrode active material has a pore structure, and a ratio K of open pores to closed pores of the negative electrode active material is 2-3.

9. The secondary battery according to claim 1, characterized in that: The negative electrode active material includes secondary particles formed by aggregation of primary particles, and the number N of primary particles in a single secondary particle is 40 to 60.

10. An electrical device, characterized in that: It comprises the secondary battery according to any one of claims 1 to 9, wherein the secondary battery is used as a power supply for the electrical equipment.

Citation Information

Patent Citations

  • Silicon-based negative electrode conductive network system, and preparation method and application thereof

    CN113363428A

  • Positive electrode for secondary battery and nonaqueous electrolyte secondary battery using the same

    JP2009129889A

  • Electrode for battery

    JP2013016515A