Lithium ion conductive solid electrolyte based on sulfide and preparation method thereof
By melt-quenching Li2S, B2S3, B2O3 and LiX in a combination of specific molar ratios, glass solid electrolytes with high thermal stability and high ionic conductivity are prepared, which solves the thermal stability and conductivity of existing materials. Deficiencies, suitable for solid-state lithium-ion batteries.
Patent Information
- Application Number
- CN202380034850.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-04
- Filing Date
- 2023-05-03
- Publication Date
- 2024-11-22
AI Technical Summary
The existing lithium-ion conductive solid electrolyte materials have shortcomings in thermal stability and ionic conductivity, and it is difficult to achieve both high thermal stability and high ionic conductivity at the same time.
通过将Li2S、B2S3、B2O3和LiX以特定摩尔比的组合进行熔融淬火,制备出具有高热稳定性和高离子电导率的玻璃态固体电解质材料,具体步骤包括混合物的热处理和淬火以获得固体材料。
The high thermal stability of the material is achieved by a high ΔTx greater than 100°C and high ionic conductivity. Combined with low electronic conductivity, it is suitable for solid-state lithium-ion battery electrolytes, improving the safety and performance of the battery.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] Technical Field and Background Art
[0002] The present invention relates to a solid material obtainable by melt quenching a mixture of lithium sulfide, boron sulfide and boron oxide to form a glassy solid suitable for use as a lithium ion conducting electrolyte. The present invention also relates to a method for preparing the solid material, an electrochemical cell such as a solid-state battery comprising the solid material and the use of the solid material in an electrochemical cell such as a solid-state battery, in particular as an electrolyte.
[0003] The three main functional components of a lithium-ion battery are the anode, cathode, and electrolyte. Although there are many variations, the anode of a conventional lithium-ion battery is usually made of carbon, the cathode is usually made of a transition metal oxide (particularly oxides of cobalt, nickel, and / or manganese), and the electrolyte is usually a non-aqueous solvent containing a lithium salt. For example, a mixture of an organic carbonate and lithium hexafluorophosphate is a well-known liquid electrolyte for lithium-ion batteries.
[0004] A significant disadvantage of liquid electrolytes is that the constituent components, especially the solvents, are flammable, which poses a significant safety risk during normal operation and especially in the event of an accident. Another disadvantage is inherent to the liquid nature of the electrolyte, which is associated with an increased risk of leakage and of environmental contamination in the event of a spill or leak.
[0005] Recently, efforts have been made to develop solid electrolytes that allow solid-state lithium-ion batteries to be provided. Such solid-state batteries have significantly reduced EHS (environmental, health and safety) hazards. An emerging class of lithium-ion conducting solid electrolytes are sulfide-based amorphous solids (interchangeably referred to as glassy solids), such as Li2S-SiS2, Li2S-P2S5 or Li2S-B2S3. In glassy solid electrolyte materials, the lack of crystallization paths leads to isotropic conduction with essentially no grain boundary resistance. The absence of grain boundaries in glassy electrolyte materials can also prevent dendrite formation, because glassy amorphous electrolyte materials can be obtained as dense, defect-free films by melt-quenching methods.
[0006] The main challenge in producing glassy solid electrolytes is to avoid crystalline regions in the solid material. The thermal stability of glass, ΔT x It can be characterized as the stability against crystallization, which is determined by the onset of crystallization (T x ) and glass transition temperature (T g ) is determined by the temperature difference between x = T x -T g . Larger ΔT x Often associated with improved glass forming ability and increased glass stability during post-processing.
[0007] Early studies on Li2S-B2S3 compositions with molar ratios of 70:30 and 60:40 reported ΔT x The values are about 70°C and about 110°C, respectively (Zhang et al., Solid State Ionics 1990, 38, 217-224).
[0008] US5500291 considers sulfide-based lithium ion conducting solid electrolytes of the Li2S-SiS2-Li4SiO4 type.
[0009] WO2020 / 254314 A1 considers sulfide-based lithium ion conducting solid electrolytes of the Li2S-B2S3 type obtained from mixtures also containing P, Si, Ge, As or Sb oxides in combination with lithium halides. The resulting glassy solids are said to have favorable lithium ion conductivity as well as electrochemical stability in direct contact with lithium metal and chemical stability to air and moisture. The ΔT of these solids x In the range of 5°C to 36°C (Table 3 of WO2020 / 254314 A1).
[0010] WO2016 / 089899 A1 considers a large number of glass systems (many of which are speculative or unproven). Paragraphs 186 and 188 of WO2016 / 089899 A1 suggest adding oxygen to improve ΔT x WO2016 / 089899 A1, paragraph 190, speculates that a system based on Li2S / Li2O-B2S3-SiS2 can have a ΔT greater than 100°C. x .
[0011] A drawback associated with most sulfide-based lithium-ion conducting solid electrolytes known in the art is that they either have low ionic conductivity or high ΔT x Therefore, there is a great need to provide sulfide-based lithium-ion conducting solid electrolytes that combine these two properties.
[0012] The object of the present invention is to provide a x , especially ΔT greater than 100°C x A sulfide-based lithium ion conductive solid electrolyte. Another object of the present invention is to provide a sulfide-based lithium ion conductive solid electrolyte having high ionic conductivity. Another object of the present invention is to provide a sulfide-based lithium ion conductive solid electrolyte having low conductivity. Summary of the invention
[0013] The present inventors have found that one or more of the objects of the present invention can be achieved by providing a sulfide-based lithium ion conducting solid electrolyte which can be obtained by melt quenching a combination of Li2S; B2S3; B2O3 and LiX in a well-defined ratio, wherein X represents Cl, Br, I or a combination thereof. As shown in the accompanying examples, it is actually observed that the resulting glassy solid exhibits a high thermal stability ΔT of Li-S-based glasses. x , high ionic conductivity and / or low electrical conductivity.
[0014] Implementation 1
[0015] Therefore, in a first aspect of the present invention, there is provided a solid material having a composition according to general formula (I)
[0016] Li 2c+d B 2a+2b S 3a+c O 3b X d (I)
[0017] in
[0018] X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof;
[0019] a is in the range of 0.03 to 0.1;
[0020] b is in the range of 0 to 0.04;
[0021] c is in the range of 0.12 to 0.26; and
[0022] d is in the range of 0.001 to 0.14.
[0023] Preferably, a solid material is provided, the solid material having a composition according to general formula (I)
[0024] Li 2c+d B 2a+2b S 3a+c O 3b X d (I)
[0025] in
[0026] X represents Cl, Br, I or a combination thereof;
[0027] a is in the range of 0.03 to 0.1;
[0028] b is in the range of 0 to 0.04;
[0029] c is in the range of 0.12 to 0.26; and
[0030] d is in the range of 0.001 to 0.14.
[0031] Implementation 2
[0032] In another aspect of the present invention, a solid material is provided, which can be obtained by melting and quenching a mixture of A and B.
[0033] wherein the molar ratio of A to B in the mixture before quenching is in the range of 60:40 to 99:1;
[0034] Wherein component A conforms to the general formula (II)
[0035] xLi2S-yB2S3-zB2O3(II)
[0036] in
[0037] x is in the range of 55 to 85;
[0038] y is in the range of 15 to 45;
[0039] z ranges from 0 to 15;
[0040] x+y+z = 100; and
[0041] Wherein component B is LiX, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof, preferably X represents Cl, Br, I or a combination thereof.
[0042] Implementation 3
[0043] In another aspect of the present invention, there is provided a method for preparing a solid material, the method comprising the following steps:
[0044] (i) providing the following precursors:
[0045] •Li2S;
[0046] • B2S3 and / or both boron and sulfur;
[0047] • optionally B2O3; and
[0048] •LiX, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof, preferably X represents Cl, Br, I or a combination thereof;
[0049] (ii) preparing a mixture comprising the precursor provided in step (i), wherein
[0050] • In the mixture, the molar ratio of the elements Li, S, B, O and X conforms to the general formula (I)
[0051] Li 2c+d B 2a+2b S 3a+c O 3b X d (I)
[0052] in
[0053] a is in the range of 0.03 to 0.1;
[0054] b is in the range of 0 to 0.04;
[0055] c is in the range of 0.12 to 0.26; and
[0056] d is in the range of 0.001 to 0.14;
[0057] or
[0058] • In the mixture, the molar ratio of the precursors conforms to the general formula (II)
[0059] xLi2S-yB2S3-zB2O3(II)
[0060] in
[0061] x is in the range of 55 to 85;
[0062] y is in the range of 15 to 45;
[0063] z is in the range of 0 to 15; and
[0064] x+y+z = 100
[0065] (iii) heat treating the mixture prepared in step (ii) to obtain a melt; and
[0066] (iv) quenching the melt obtained in step (iii) to obtain the solid material.
[0067] Implementation 4
[0068] In another aspect of the present invention, a solid composition is provided, which comprises a first solid material, which is a solid material as described herein (i.e., the solid material of Embodiment 1 or 2), and further comprises at least a second solid material, which has a composition different from that of the first solid material.
[0069] Implementation 5
[0070] In another aspect of the present invention, an electrochemical cell is provided, the electrochemical cell comprising the solid material as described herein (ie the solid material of Embodiment 1 or 2).
[0071] Implementation 6
[0072] In another aspect of the present invention, there is provided use of a solid material as described herein (ie, the solid material of Embodiment 1 or 2) or a solid composition as described herein (ie, the solid composition of Embodiment 4) as a solid electrolyte for an electrochemical cell.
[0073] Implementation Plan 7
[0074] Another aspect of the present invention relates to a battery, more particularly a lithium ion battery or a lithium metal battery, comprising at least one electrochemical cell comprising a solid material as described herein (i.e., the solid material of Embodiment 1 or 2), for example two or more electrochemical cells as described in Embodiment 5.
[0075] Implementation 8
[0076] Another aspect of the invention is a method of manufacturing or operating an automobile, a computer, a personal digital assistant, a mobile phone, a watch, a camcorder, a digital camera, a thermometer, a calculator, a laptop BIOS, a communication device, a remote car lock, and a stationary application (such as an energy storage device for a power plant) by using at least one battery or at least one electrochemical cell comprising a solid material as described herein (i.e., an electrochemical cell as described in Embodiment 5).
[0077] Implementation Plan 9
[0078] Another aspect of the present disclosure is the use of an electrochemical cell comprising the solid material of the present invention (i.e., an electrochemical cell as described in Embodiment 5) in a motor vehicle, a bicycle operated by an electric motor, a robot, an aircraft (e.g., an unmanned aerial vehicle including a drone), a ship, or a stationary energy storage device.
[0079] Implementation 10
[0080] In another aspect of the present invention, a lithium salt of formula LiX is provided for improving the thermal stability ΔT of a glassy solid. x , especially for improving the thermal stability ΔT of sulfide-based lithium-ion conducting solid electrolytes x The use of, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof, preferably X represents Cl, Br, I or a combination thereof. DETAILED DESCRIPTION
[0081] In the following specific embodiments, preferred embodiments are described in detail to practice the present invention. Although the present invention is described with reference to these specific preferred embodiments, it should be understood that the present invention is not limited to these preferred embodiments. On the contrary, the present invention includes many substitutions, modifications and equivalent forms, which will become apparent by considering the following specific embodiments.
[0082] As referred to herein, the glass transition temperature (T g ) refers to the temperature at which the glass transition starts as determined by differential scanning calorimetry (DSC). The glass transition temperature is preferably determined by constructing tangents to the DSC curve baseline before and after the glass transition and determining the extrapolated starting temperature by the intersection of these tangents, which corresponds substantially to the temperature at which the highest slope of the DSC baseline decreases before the exothermic crystallization peak. The DSC is preferably recorded using the following temperature profile: from 100°C to 350°C at a rate of 10°C / min, and preferably on a 5mg to 10mg sample in a sealed aluminum pan. A suitable DSC apparatus is a DSC 3500 Sirius.
[0083] As referred to herein, thermal stability (ΔT x ) is the crystallization onset temperature (T x ) and the glass transition temperature (T g ). In other words: ΔT x = T x – T g As explained in the previous paragraph, the glass transition temperature (T g ) refers to the temperature of the onset of glass transition determined by differential scanning calorimetry (DSC).
[0084] As referred to herein, ionic conductivity refers to the ionic conductivity determined by electrochemical impedance spectroscopy (EIS) at 25°C. The ionic conductivity is preferably measured with an ion blocking electrode on a hot pressed sample densified at 125°C for 5 min at 350 MPa, after which the ionic conductivity is measured at 25°C at an operating pressure of 125 MPa. Preferably, an excitation voltage of 10 mV is applied in the frequency range of 7 MHz to 1 Hz, and the data are interpreted by equivalent circuit analysis. A suitable conductivity analyzer is a potentiostat with a frequency analyzer (such as available from Biologic).
[0085] The electronic conductivity as referred to herein refers to the electronic conductivity determined at 25°C. The electronic conductivity is preferably measured with an ion blocking electrode on a hot pressed sample densified at 125°C for 5 min at 350 MPa, after which the electronic conductivity is measured at 25°C at an operating pressure of 125 MPa. Preferably, the electronic conductivity is measured via stepwise potentiostatic polarization at 0.2V, 0.4V and 0.6V for 20 min. A suitable conductivity analyzer is a potentiostat with a frequency analyzer such as available from Biologic.
[0086] Implementation 1
[0087] In a first aspect of the present invention, there is provided a solid material having a composition according to general formula (I)
[0088] Li 2c+d B 2a+2b S 3a+c O 3b X d (I)
[0089] in
[0090] X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4, or a combination thereof;
[0091] a is in the range of 0.03 to 0.1;
[0092] b is in the range of 0 to 0.04;
[0093] c is in the range of 0.12 to 0.26; and
[0094] d is in the range of 0.001 to 0.14.
[0095] Without wishing to be bound by any theory, the inventors believe that the solid material according to formula (I) is the result obtained when a mixture Li2S; B2S3; B2O3 and LiX is melt-quenched in a well-defined ratio, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof, as explained herein in the context of other aspects of the invention and in the examples.
[0096] Preferably there is provided a solid material having a composition according to the general formula (I)
[0097] in
[0098] X represents Cl, Br, I or a combination thereof;
[0099] a is in the range of 0.03 to 0.1;
[0100] b is in the range of 0 to 0.04;
[0101] c is in the range of 0.12 to 0.26; and
[0102] d is in the range of 0.001 to 0.14.
[0103] Preferably a solid material having a composition according to general formula (I) is provided, wherein
[0104] a is in the range of 0.06 to 0.1;
[0105] b is in the range of 0 to 0.03;
[0106] c is in the range of 0.12 to 0.20; and
[0107] d is in the range of 0.001 to 0.14;
[0108] More preferably,
[0109] a is in the range of 0.06 to 0.1;
[0110] b is in the range of 0.002 to 0.02;
[0111] c is in the range of 0.14 to 0.19; and
[0112] d is in the range of 0.001 to 0.14.
[0113] Generally, it is preferred that d is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04. In some embodiments, d is in the range of 0.01 to 0.14, preferably in the range of 0.02 to 0.14, more preferably in the range of 0.025 to 0.14. In some embodiments, d is in the range of 0.02 to 0.0.08, preferably in the range of 0.025 to 0.08, more preferably in the range of 0.03 to 0.07.
[0114] Thus, in some embodiments of the present invention, there is provided a solid material having a composition according to formula (I), wherein
[0115] a is in the range of 0.06 to 0.1;
[0116] b is in the range of 0 to 0.03;
[0117] c is in the range of 0.12 to 0.20; and
[0118] d is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04;
[0119] More preferably,
[0120] a is in the range of 0.06 to 0.1;
[0121] b is in the range of 0.002 to 0.02;
[0122] c is in the range of 0.14 to 0.19; and
[0123] d is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04.
[0124] According to a highly preferred embodiment of the present invention, there is provided a solid material having a composition according to general formula (I), wherein
[0125] a is in the range of 0.06 to 0.8, preferably in the range of 0.07 to 0.09;
[0126] b is in the range of 0.002 to 0.02, preferably in the range of 0.010 to 0.015;
[0127] c is in the range of 0.11 to 0.21, preferably in the range of 0.14 to 0.18; and
[0128] d is in the range of 0.001 to 0.13, preferably in the range of 0.02 to 0.06.
[0129] Thus, in some embodiments of the present invention, there is provided a solid material having a composition according to formula (I), wherein
[0130] a ranges from 0.07 to 0.09;
[0131] b is in the range of 0.010 to 0.015
[0132] c is in the range of 0.14 to 0.18; and
[0133] d is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04.
[0134] In a highly preferred embodiment of the present invention, the solid material conforms to formula (I), wherein X represents a combination of Cl, Br and / or I. In other words, the solid material according to the present invention conforms to formula (I)a, formula (I)b, formula (I)c or formula (I)d, wherein
[0135] a is in the range of 0.03 to 0.1;
[0136] b is in the range of 0 to 0.04;
[0137] c is in the range of 0.12 to 0.26; and
[0138] d is in the range of 0.001 to 0.14
[0139] Formula (I)a <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b (BrCl) d ]]> Formula (I)b <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b (BRI) d ]]> Formula (I)c <![CDATA[Li 2c+d B 2a+2b S 3a+c HE 3b (Cl) d ]]> Formula (I)d <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b (ClBrI) d ]]>
[0140] As will be appreciated by the skilled artisan, all embodiments relating to formula (I) are equally applicable to formula (I)a, formula (I)b, formula (I)c and formula (I)d.
[0141] In certain preferred embodiments, the solid material of the present invention conforms to formula (I):
[0142] Li 2c+d B 2a+2b S 3a+c O 3b Y 1 e Y 2 f (I)'
[0143] where Y 1 and Y 2 is independently selected from the group consisting of: F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4, and Y 1 ≠Y 2 ;and
[0144] in
[0145] a is in the range of 0.03 to 0.1;
[0146] b is in the range of 0 to 0.04;
[0147] c is in the range of 0.12 to 0.26;
[0148] e is in the range of 0.001 to 0.14; and
[0149] f is in the range of 0.001 to 0.14.
[0150] In a preferred embodiment, Y 1 and Y 2 Independently selected from the group consisting of Cl, Br and I.
[0151] Preferably, the solid material conforms to formula (I)', wherein
[0152] a is in the range of 0.06 to 0.1;
[0153] b is in the range of 0.002 to 0.02;
[0154] c ranges from 0.14 to 0.19;
[0155] e is in the range of 0.001 to 0.14; and
[0156] f is in the range of 0.001 to 0.14.
[0157] Preferably, the solid material conforms to formula (I)', wherein
[0158] e is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04; and
[0159] f is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, and more preferably in the range of 0.01 to 0.04.
[0160] In highly preferred embodiments, the solid material conforms to Formula (I)'a, Formula (I)'b or Formula (I)'c
[0161] Formula (I)'a <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b Br e Cl f ]]> Formula (I)'b <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b Br e I f ]]> Formula (I)'c <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b Cl e I f ]]>
[0162] As will be appreciated by the skilled artisan, all embodiments relating to Formula (I)' are equally applicable to Formula (I)'a, Formula (I)'b and Formula (I)'c.
[0163] In certain preferred embodiments, the solid material of the present invention conforms to formula (I):
[0164] Li 2c+d B 2a+2b S 3a+c O 3b Y 3 g Y 4 h Y 5 i (I)''
[0165] where Y 3 , Y 4 and Y 5 is independently selected from the group consisting of: F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4, and Y 3 ≠Y 4 ≠Y 5 ;and
[0166] in
[0167] a is in the range of 0.03 to 0.1;
[0168] b is in the range of 0 to 0.04;
[0169] c is in the range of 0.12 to 0.26;
[0170] g is in the range of 0.001 to 0.14;
[0171] h is in the range of 0.001 to 0.14; and
[0172] i is in the range of 0.001 to 0.14.
[0173] In a preferred embodiment, Y 3 , Y 4 and Y 5 Independently selected from the group consisting of Cl, Br and I.
[0174] Preferably, the solid material conforms to formula (I)'', wherein
[0175] a is in the range of 0.06 to 0.1;
[0176] b is in the range of 0.002 to 0.02;
[0177] c ranges from 0.14 to 0.19;
[0178] g is in the range of 0.001 to 0.14;
[0179] h is in the range of 0.001 to 0.14; and
[0180] i is in the range of 0.001 to 0.14.
[0181] Preferably, the solid material conforms to formula (I)'', wherein
[0182] g is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04;
[0183] h is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04; and
[0184] i is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.04.
[0185] In a highly preferred embodiment, the solid material conforms to formula (I):
[0186] Formula (I)"a <![CDATA[Li 2c+d B 2a+2b S 3a+c O 3b Br g Cl h I i ]]>
[0187] As will be appreciated by the skilled person, all embodiments relating to formula (I)'' are equally applicable to formula (I)''a.
[0188] In each embodiment of the composition according to formula (I) described herein, the molar ratios have been calculated such that the sum of 5a+5b+3c+2d is in the range of 0.9 to 1.1, preferably in the range of 0.99 to 1.01, and most preferably is about 1. In addition, in each embodiment of the composition according to formula (I)' or formula (I)'' described herein, the molar ratios have been calculated such that the sum of 5a+5b+3c+2d is in the range of 0.9 to 1.1, preferably in the range of 0.99 to 1.01, and most preferably is about 1.
[0189] A solid material having a composition according to general formula (I), if prepared by, for example, melt quenching, may be accompanied by a small amount of impurity phases, which are usually mainly composed of a precursor used to prepare the solid material or an intermediate formed from the precursor. In addition, a solid material having a composition according to general formula (I)' or general formula (I)'', if prepared by, for example, melt quenching, may be accompanied by a small amount of impurity phases, which are usually mainly composed of a precursor used to prepare the solid material or an intermediate formed from the precursor.
[0190] Implementation 2
[0191] In another aspect of the present invention, a solid material is provided, which can be obtained by melting and quenching a mixture of A and B.
[0192] wherein the molar ratio of A to B in the mixture before quenching is in the range of 60:40 to 99:1;
[0193] Wherein component A conforms to the general formula (II)
[0194] xLi2S-yB2S3-zB2O3(II)
[0195] in
[0196] x is in the range of 55 to 85, preferably in the range of 55 to 75, more preferably in the range of 60 to 70;
[0197] y is in the range of 15 to 45, preferably in the range of 20 to 40, more preferably in the range of 25 to 35;
[0198] z is in the range of 0 to 15, preferably in the range of 0 to 10, more preferably in the range of 0 to 6;
[0199] x+y+z = 100; and
[0200] Wherein component B is LiX, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof.
[0201] In a preferred embodiment of the present invention, the solid material can be obtained by melting and quenching a mixture of A and B.
[0202] wherein the molar ratio of A to B in the mixture before quenching is in the range of 60:40 to 99:1;
[0203] Wherein component A conforms to the general formula (II)
[0204] xLi2S-yB2S3-zB2O3(II)
[0205] in
[0206] x is in the range of 55 to 85, preferably in the range of 55 to 75, more preferably in the range of 60 to 70;
[0207] y is in the range of 15 to 45, preferably in the range of 20 to 40, more preferably in the range of 25 to 35;
[0208] z is in the range of 0 to 15, preferably in the range of 0 to 10, more preferably in the range of 0 to 6;
[0209] x+y+z = 100; and
[0210] Wherein component B is LiX, wherein X represents Cl, Br, I or a combination thereof.
[0211] In a preferred embodiment of the present invention, there is provided the solid material obtainable by melt quenching a mixture of A and B, wherein
[0212] x is in the range of 62 to 68, preferably in the range of 63 to 67, more preferably in the range of 64 to 66;
[0213] y is in the range of 27 to 33, preferably in the range of 28 to 32, more preferably in the range of 29 to 31;
[0214] z is in the range of 1 to 8, preferably in the range of 3 to 7, more preferably in the range of 4 to 6; and
[0215] x+y+z = 100.
[0216] According to a highly preferred embodiment of the present invention, there is provided a solid material obtainable by melt quenching a mixture of A and B, wherein
[0217] x is about 65;
[0218] y is about 30; and
[0219] z is about 5.
[0220] Generally, preferably, the molar ratio of A to B in the mixture before quenching is in the range of 75:25 to 98:2, preferably in the range of 80:20 to 96:4, and more preferably in the range of 85:15 to 96:4. In some embodiments, the molar ratio of A to B in the mixture before quenching is in the range of 60:40 to 96:4, preferably in the range of 70:30 to 96:4, and more preferably in the range of 75:25 to 96:4. In some embodiments, the molar ratio of A to B in the mixture before quenching is in the range of 60:40 to 94:6, preferably in the range of 70:30 to 93:7, and more preferably in the range of 75:25 to 92:8.
[0221] Thus, in some embodiments of the present invention, there is provided a solid material obtainable by melt quenching a mixture of A and B, wherein
[0222] x is in the range of 62 to 68, preferably in the range of 63 to 67, more preferably in the range of 64 to 66;
[0223] y is in the range of 27 to 33, preferably in the range of 28 to 32, more preferably in the range of 29 to 31;
[0224] z is in the range of 1 to 8, preferably in the range of 3 to 7, more preferably in the range of 4 to 6;
[0225] x+y+z = 100; and
[0226] The molar ratio of A to B in the mixture before quenching is in the range of 75:25 to 98:2, preferably in the range of 80:20 to 96:4, more preferably in the range of 85:15 to 96:4.
[0227] In some embodiments of the present invention, there is provided a solid material obtainable by melt quenching a mixture of A and B, wherein
[0228] x is about 65;
[0229] y is about 30;
[0230] z is about 5;
[0231] x+y+z = 100; and
[0232] The molar ratio of A to B in the mixture before quenching is in the range of 75:25 to 98:2, preferably in the range of 80:20 to 96:4, more preferably in the range of 85:15 to 96:4.
[0233] In another aspect of the present invention, a solid material is provided, which can be obtained by melting and quenching a mixture of A, B and C.
[0234] wherein the molar ratio of A, B and C in the mixture before quenching is in the range of 40:30:30 to 98:1:1;
[0235] Wherein component A conforms to the general formula (II)
[0236] xLi2S-yB2S3-zB2O3(II)
[0237] in
[0238] x is in the range of 55 to 85, preferably in the range of 55 to 75, more preferably in the range of 60 to 70;
[0239] y is in the range of 15 to 45, preferably in the range of 20 to 40, more preferably in the range of 25 to 35;
[0240] z is in the range of 0 to 15, preferably in the range of 0 to 10, more preferably in the range of 0 to 6;
[0241] x+y+z = 100; and
[0242] Wherein component B is LiY 6 , Y 6 represents Br, Cl, I or a combination thereof, preferably Y 6 represents Br, Cl or I;
[0243] Where component C is LiY 7 , where Y 7 represents Br, Cl, I or a combination thereof, preferably wherein Y 7 represents Br, Cl or I; and
[0244] where Y 6 ≠Y 7 .
[0245] In a preferred embodiment of the present invention, there is provided said solid material obtainable by melt quenching a mixture of A, B and C, wherein
[0246] x is in the range of 62 to 68, preferably in the range of 63 to 67, more preferably in the range of 64 to 66;
[0247] y is in the range of 27 to 33, preferably in the range of 28 to 32, more preferably in the range of 29 to 31;
[0248] z is in the range of 1 to 8, preferably in the range of 3 to 7, more preferably in the range of 4 to 6; and
[0249] x+y+z = 100.
[0250] According to a highly preferred embodiment of the present invention, there is provided a solid material obtainable by melt quenching a mixture of A, B and C, wherein
[0251] x is about 65;
[0252] y is about 30; and
[0253] z is about 5.
[0254] Generally, preferably, the molar ratio of A, B and C in the mixture before quenching is in the range of 50:25:25 to 98:1:1, preferably in the range of 56:22:22 to 90:5:5, more preferably in the range of 64:15:21 to 80:10:10. In some embodiments, the molar ratio of A, B and C in the mixture before quenching is in the range of 60:20:20 to 95:3:2, preferably in the range of 70:15:15 to 90:5:5, more preferably in the range of 76:12:12 to 82:9:9. In some highly preferred embodiments, the molar ratio of A, B and C in the mixture before quenching is in the range of 50:25:25 to 96:2:2, preferably in the range of 60:20:20 to 90:5:5, more preferably in the range of 70:15:15 to 80:10:10.
[0255] Without wishing to be bound by any theory, it is believed that generally and therefore in some preferred embodiments of the present invention, the solid material obtainable by melt-quenching a mixture of A and B as described herein is a solid material having a composition according to general formula (I) as described herein (i.e. the solid material of Embodiment 1).
[0256] The solid materials according to different aspects of the present invention described herein, i.e., the solid materials having a composition according to general formula (I) as described herein (i.e., the solid materials of Embodiment 1) and the solid materials obtainable by melt-quenching the mixture of A and B as described herein (i.e., the solid materials of Embodiment 2), are collectively referred to as "solid materials" (i.e., the solid materials of Embodiment 1 or 2).
[0257] According to a preferred embodiment of the present invention, there is provided a solid material wherein X represents Br, I or a combination thereof. As shown in the accompanying examples, these materials have a thermal stability ΔT x In this aspect, it is superior to the material in which X represents Cl.
[0258] According to a preferred embodiment of the present invention, a solid material is provided wherein at least 50 mol % of X represents Br, preferably at least 80 mol % of X represents Br, and most preferably X represents Br. As shown in the accompanying examples, the material wherein X represents Br has a thermal stability ΔT x In this aspect, it is superior to the material in which X represents Cl.
[0259] According to a preferred embodiment of the present invention, a solid material is provided, wherein X represents Br, I or a combination thereof, and wherein at least 50 mol % of X represents Br, preferably at least 80 mol % of X represents Br.
[0260] The solid material of the present invention is generally a glassy solid that can be obtained by melting and quenching a precursor mixture as explained elsewhere herein. In some embodiments, the solid material is in the form of a single sheet of glass, such as a single sheet of glass melt-cast. Preferably, the glassy solid is substantially free of a crystalline phase. This may mean that in some embodiments, the amount of the crystalline phase determined by X-ray diffraction is less than 5 volume %, preferably less than 2 volume %, more preferably less than 1 volume % of the solid material. If the reflection intensity of the phase is higher than the background by more than 10%, it is considered that the phase is crystalline.
[0261] The solid materials of the present invention are found to have surprisingly high ionic conductivity. According to a preferred embodiment of the present invention, a solid material is provided, wherein the material has an ionic conductivity of at least 0.1 mS / cm, preferably at least 0.3 mS / cm at 25°C. As shown in the accompanying examples, the inventors have surprisingly found that when at least 50 mol% of X represents Br, preferably at least 80 mol% of X represents Br, and most preferably X represents Br, the ionic conductivity at 25°C can be as high as 1.2 mS / cm. Therefore, in some embodiments of the present invention, a solid material is provided, wherein the material has an ionic conductivity of at least 1 mS / cm, preferably at least 1.1 mS / cm, more preferably at least 1.2 mS / cm at 25°C. In a specific embodiment of the present invention, wherein the solid material of the present invention:
[0262] - at least 50 mol % of X represent Br, preferably at least 80 mol % of X represent Br, most preferably X represents Br; and
[0263] - The ionic conductivity at 25°C is at least 1 mS / cm, preferably at least 1.1 mS / cm, more preferably at least 1.2 mS / cm.
[0264] For example, in some embodiments of the solid material of the invention, at least 80 mol% of X represents Br, and the solid material has an ionic conductivity of at least 1.1 mS / cm at 25°C, or X represents Br, and the solid material has an ionic conductivity of at least 1.2 mS / cm at 25°C, such as at least 1.21 mS / cm or at least 1.25 mS / cm.
[0265] The solid materials of the present invention are found to combine the high ionic conductivity with surprisingly low electronic conductivity, which makes them very attractive solid-state battery electrolyte materials. According to a preferred embodiment of the present invention, a solid material is provided, wherein the material has a conductivity of less than 1×10 -4 mS / cm, preferably less than 6×10 -5 As shown in the accompanying examples, the inventors have surprisingly found that when X represents Br, I or a combination thereof, the electronic conductivity at 25°C can be very low, such as less than 1×10 -9 mS / cm or less than 1×10 -10 mS / cm. Therefore, in some embodiments of the present invention, a solid material is provided, wherein the material has a relative humidity of less than 1×10 -5 mS / cm, preferably less than 1×10 -6 mS / cm electronic conductivity. In a specific embodiment of the present invention:
[0266] -X represents Br, I or a combination thereof; and
[0267] - Solid materials have a temperature of less than 1×10 -9 mS / cm or less than 1×10 -10 Electronic conductivity in mS / cm.
[0268] In some particularly preferred embodiments of the present invention, materials are provided that combine high ionic conductivity with low electronic conductivity. As shown in the accompanying examples, this is possible when X represents Br. For example, in some embodiments of the solid material of the present invention:
[0269] - at least 50 mol % of X represent Br, preferably at least 80 mol % of X represent Br, most preferably X represents Br;
[0270] - the solid material has an ionic conductivity at 25°C of at least 1 mS / cm, preferably at least 1.1 mS / cm, more preferably at least 1.2 mS / cm; and
[0271] - Solid materials have a temperature of less than 1×10 -9 mS / cm or less than 1×10-10 Electronic conductivity in mS / cm.
[0272] For example, in some embodiments, at least 50 mol% of X represents Br, preferably at least 80 mol% of X represents Br, and most preferably X represents Br; the solid material has an ionic conductivity of at least 1.2 mS / cm at 25°C, and the solid material has an ionic conductivity of less than 1×10 -10 Electronic conductivity in mS / cm.
[0273] As shown in the accompanying examples, it was found that the glassy solid of the present invention exhibits a high thermal stability ΔT for Li-S based glasses. x According to a preferred embodiment of the present invention, a solid material is provided, wherein the material has a thermal stability ΔT greater than 100°C, preferably greater than 110°C, more preferably greater than 115°C. x In some embodiments, particularly when X represents Br, I, or a combination thereof, the thermal stability ΔT x Greater than 120°C, preferably greater than 125°C, more preferably greater than 130°C.
[0274] In certain highly preferred embodiments, there is provided a solid material of the invention wherein
[0275] - the solid material has an ionic conductivity at 25°C of at least 0.1 mS / cm, preferably at least 0.3 mS / cm;
[0276] - The solid material has a thermal stability ΔT greater than 100°C, preferably greater than 110°C, more preferably greater than 115°C x ;and
[0277] - Preferably the solid material has a temperature of less than 1×10 -5 mS / cm, preferably less than 1×10 -6 Electronic conductivity in mS / cm.
[0278] In certain highly preferred embodiments, there is provided a solid material of the invention wherein
[0279] - at least 50 mol % of X represent Br, preferably at least 80 mol % of X represent Br, most preferably X represents Br;
[0280] - the solid material has an ionic conductivity at 25°C of at least 1 mS / cm, preferably at least 1.1 mS / cm, more preferably at least 1.2 mS / cm;
[0281] - the solid material has a thermal stability ΔT greater than 120°C, preferably greater than 125°C, more preferably greater than 130°C x ;and
[0282] - Preferably the solid material has a temperature of less than 1×10 -9 mS / cm or less than 1×10 -10 Electronic conductivity in mS / cm.
[0283] For example, in some embodiments, X represents I or Br, preferably Br; - the solid material has an ionic conductivity of at least 1.1 mS / cm, more preferably at least 1.2 mS / cm at 25°C; and the solid material has a thermal stability ΔT greater than 115°C, preferably greater than 125°C x .
[0284] Without wishing to be bound by any theory, it is believed that generally and therefore in some preferred embodiments of the present invention, the solid material obtainable by melt quenching a mixture of A, B and C as described herein is a solid material having a composition according to general formula (I) as described herein.
[0285] The solid materials according to the different aspects of the present invention described herein, i.e. the solid materials having a composition according to general formula (I)' as described herein and the solid materials obtainable by melt quenching a mixture of A, B and C as described herein, are collectively referred to as "solid materials".
[0286] According to a preferred embodiment of the present invention, there is provided a solid material conforming to the general formula (I)', wherein Y 1 represents Br, and Y 2 represents Cl,
[0287] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0288] At least 50 mol% of Y 2 represents Cl, preferably at least 80 mol% Y 2 represents Cl, more preferably Y 2 Indicates Cl.
[0289] The solid material of the present invention is found to have surprisingly high ionic conductivity. According to a preferred embodiment of the present invention, there is provided a solid material conforming to formula (I)', wherein the material has an ionic conductivity of at least 0.1 mS / cm, preferably at least 0.2 mS / cm at 25°C. As shown in the accompanying examples, the inventors have surprisingly found that if
[0290] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y1 represents Br, more preferably Y 1 represents Br, and
[0291] At least 50 mol% of Y 2 represents Cl, preferably at least 80 mol% Y 2 represents Cl, more preferably Y 2 represents Cl, then
[0292] The ionic conductivity at 25°C can be as high as 0.67 mS / cm.
[0293] Thus, in some embodiments of the present invention, a solid material is provided, wherein the material has an ionic conductivity at 25°C of at least 0.3 mS / cm, preferably at least 0.40 mS / cm, more preferably at least 0.49 mS / cm.
[0294] In a particular embodiment of the present invention, wherein the solid material of the present invention:
[0295] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0296] At least 50 mol% of Y 2 represents Cl, preferably at least 80 mol% Y 2 represents Cl, more preferably Y 2 represents Cl, and
[0297] The ionic conductivity at 25° C. is at least 0.40 mS / cm, preferably at least 0.50 mS / cm, more preferably at least 0.54 mS / cm.
[0298] According to a preferred embodiment of the present invention, there is provided a solid material conforming to formula (I)',
[0299] At least 50 mol% of Y 1 represents Cl, preferably at least 80 mol% Y 1 represents Cl, more preferably Y 1 represents Cl, and
[0300] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 Indicates I.
[0301] As shown in the accompanying examples, the inventors have surprisingly found that if
[0302] At least 50 mol% of Y 1 represents Cl, preferably at least 80 mol% Y 1 represents Cl, more preferably Y 1 represents Cl, and
[0303] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 If I is
[0304] The ionic conductivity at 25°C can be as high as 0.67 mS / cm.
[0305] Thus, in some embodiments of the present invention, a solid material is provided, wherein the material has an ionic conductivity at 25°C of at least 0.40 mS / cm, preferably at least 0.50 mS / cm, more preferably at least 0.62 mS / cm.
[0306] In a particular embodiment of the present invention, wherein the solid material of the present invention:
[0307] At least 50 mol% of Y 1 represents Cl, preferably at least 80 mol% Y 1 represents Cl, more preferably Y 1 represents Cl, and
[0308] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 represents I, and
[0309] The ionic conductivity at 25° C. is at least 0.50 mS / cm, preferably at least 0.60 mS / cm, more preferably at least 0.62 mS / cm.
[0310] According to a preferred embodiment of the present invention, there is provided a solid material conforming to formula (I)',
[0311] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0312] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 Indicates I.
[0313] As shown in the accompanying examples, the inventors have surprisingly found that if
[0314] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0315] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 If I is
[0316] The ionic conductivity at 25° C. can be as high as 0.76 mS / cm. Therefore, in some embodiments of the present invention, a solid material is provided, wherein the material has an ionic conductivity at 25° C. of at least 0.40 mS / cm, preferably at least 0.50 mS / cm, more preferably at least 0.54 mS / cm.
[0317] The solid materials of the present invention are found to combine the high ionic conductivity with surprisingly low electronic conductivity, which makes them very attractive solid-state battery electrolyte materials. According to a preferred embodiment of the present invention, there is provided a solid material conforming to formula (I)', wherein the material has a conductivity of less than 1×10 -4 mS / cm, preferably less than 1×10 -5 As shown in the accompanying examples, the inventors have surprisingly found that if
[0318] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0319] At least 50 mol% of Y 2 represents Cl, preferably at least 80 mol% Y 2 represents Cl, more preferably Y 2 represents Cl, then
[0320] The electronic conductivity at 25°C can be very low, such as less than 1×10 -5 mS / cm or less than 8×10 -6 mS / cm.
[0321] In a specific embodiment of the invention:
[0322] At least 50 mol% of Y 1represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0323] At least 50 mol% of Y 2 represents Cl, preferably at least 80 mol% Y 2 represents Cl, more preferably Y 2 represents Cl, and
[0324] Solid materials have a temperature of less than 1.0×10 -5 Electronic conductivity in mS / cm.
[0325] According to a preferred embodiment of the present invention, there is provided a solid material conforming to formula (I)', wherein the material has a relative humidity of less than 1×10 -4 mS / cm, preferably less than 1×10 -5 As shown in the accompanying examples, the inventors have surprisingly found that if
[0326] At least 50 mol% of Y 1 represents Cl, preferably at least 80 mol% Y 1 represents Cl, more preferably Y 1 represents Cl, and
[0327] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 If I is
[0328] The electronic conductivity at 25°C can be very low, such as less than 1×10 -5 mS / cm.
[0329] In a specific embodiment of the invention:
[0330] At least 50 mol% of Y 1 represents Cl, preferably at least 80 mol% Y 1 represents Cl, more preferably Y 1 represents Cl, and
[0331] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 represents I, and
[0332] Solid materials have a temperature of less than 1.0×10 -5Electronic conductivity in mS / cm.
[0333] According to a preferred embodiment of the present invention, a solid material is provided, wherein the material has a relative humidity of less than 1×10 -4 mS / cm, preferably less than 1×10 -5 As shown in the accompanying examples, the inventors have surprisingly found that if
[0334] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br, and
[0335] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 If I is
[0336] The electronic conductivity at 25°C can be very low, such as less than 1×10 -5 mS / cm.
[0337] In a specific embodiment of the invention:
[0338] At least 50 mol% of Y 1 represents Br, preferably at least 80 mol% of Y 1 represents Br, more preferably Y 1 represents Br;
[0339] At least 50 mol% of Y 2 represents I, preferably at least 80 mol% of Y 2 represents I, more preferably Y 2 represents I; and
[0340] Solid materials have a temperature of less than 1.0×10 -4 Electronic conductivity in mS / cm.
[0341] As explained throughout this application, the solid material of the present invention can be obtained by melting and quenching the precursor mixture to obtain a glassy solid. For some applications, it may be preferred that the material is provided in the form of a particulate solid (such as a powder). This can facilitate blending with, for example, a cathode material. The solid can be obtained directly in the form of a particulate solid (such as a powder), or can be crushed (such as by grinding, grinding, etc.) into a particulate solid (such as a powder). For other applications, it may be preferred that the solid material is provided in the form of a thin sheet or film, preferably a sheet or film having a thickness of less than 500 microns, preferably less than 100 microns.
[0342] The inventors contemplate that during the synthesis, a small amount of other materials may be added in a manner that no longer complies with the general formula (I) of the resulting solid material or in a manner that no longer complies with the general formula (II); but it is possible that the change does not substantially affect the basic and novel properties of the solid material of the present invention. For the purposes of the present invention, such modifications are considered to be within the scope of the general formula (I) or (II).
[0343] Implementation 3
[0344] In another aspect of the present invention, there is provided a method for preparing a solid material, the method comprising the following steps:
[0345] (i) providing the following precursors:
[0346] •Li2S;
[0347] • B2S3 and / or both boron and sulfur;
[0348] • optionally B2O3; and
[0349] •LiX, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof;
[0350] (ii) preparing a mixture comprising the precursor provided in step (i), wherein
[0351] • In the mixture, the molar ratio of the elements Li, S, B, O and X conforms to the general formula (I)
[0352] Li 2c+d B 2a+2b S 3a+c O 3b X d (I)
[0353] in
[0354] a is in the range of 0.03 to 0.1;
[0355] b is in the range of 0 to 0.04;
[0356] c is in the range of 0.12 to 0.26; and
[0357] d is in the range of 0.001 to 0.14;
[0358] or
[0359] • In the mixture, the molar ratio of the precursors conforms to the general formula (II)
[0360] xLi2S-yB2S3-zB2O3(II)
[0361] in
[0362] x is in the range of 55 to 85;
[0363] y is in the range of 15 to 45;
[0364] z is in the range of 0 to 15; and
[0365] x+y+z = 100
[0366] (iii) heat treating the mixture prepared in step (ii) to obtain a melt; and
[0367] (iv) quenching the melt obtained in step (iii) to obtain the solid material.
[0368] In a preferred embodiment, a method for preparing a solid material is provided, the method comprising the following steps:
[0369] (i) providing the following precursors:
[0370] •Li2S;
[0371] • B2S3 and / or both boron and sulfur;
[0372] • optionally B2O3; and
[0373] •LiX, wherein X represents Cl, Br, I or a combination thereof;
[0374] (ii) preparing a mixture comprising the precursor provided in step (i), wherein
[0375] • In the mixture, the molar ratio of the elements Li, S, B, O and X conforms to the general formula (I)
[0376] Li 2c+d B 2a+2b S 3a+c O 3b X d (I)
[0377] in
[0378] a is in the range of 0.03 to 0.1;
[0379] b is in the range of 0 to 0.04;
[0380] c is in the range of 0.12 to 0.26; and
[0381] d is in the range of 0.001 to 0.14;
[0382] or
[0383] • In the mixture, the molar ratio of the precursors conforms to the general formula (II)
[0384] xLi2S-yB2S3-zB2O3(II)
[0385] in
[0386] x is in the range of 55 to 85;
[0387] y is in the range of 15 to 45;
[0388] z is in the range of 0 to 15; and
[0389] x+y+z = 100
[0390] (iii) heat treating the mixture prepared in step (ii) to obtain a melt; and
[0391] (iv) quenching the melt obtained in step (iii) to obtain the solid material.
[0392] This method is generally referred to as the melt quenching method of the present invention. The process is cost-effective and easy to scale. General formula (I), in particular the preferred embodiments of a, b, c and d described herein in the context of embodiment 1 are also applicable to the method for preparing solid materials. Similarly, general formula (II), in particular the preferred embodiments of x, y and z described herein in the context of embodiment 2 are also applicable to the melt quenching method of the present invention. In addition, the preferred embodiments of the solid materials of the present invention (i.e., embodiment 1 or 2) are generally (e.g., with respect to the identity of X, electrical conductivity, thermal stability, etc.) also applicable to the melt quenching method of embodiment 3.
[0393] Providing both boron and sulfur in step (i) should be interpreted as meaning providing elemental boron and elemental sulfur.Elemental boron and elemental sulfur may be provided in amorphous or crystalline form, wherein the specific allotrope used is not particularly limiting to the present invention.
[0394] Preparing the mixture of step (ii) may be carried out by any suitable means, preferably by mechanical milling (eg ball milling).
[0395] Step (iii) involves heating the mixture prepared in step (ii) to obtain a melt, i.e., heat treating at a temperature higher than the melting temperature of the mixture prepared in step (ii). Step (iii) preferably comprises heat treating the mixture prepared in step (ii) at a temperature of at least 400° C., preferably at least 600° C., more preferably at least 800° C. The mixture is preferably kept at this temperature for at least 15 minutes, preferably at least 30 minutes, more preferably at least 2 hours.
[0396] The heat treatment can be carried out in a closed container. The closed container can be a sealed quartz tube or any other type of container that can withstand the temperature of the heat treatment and does not react with the components of the glass, such a closed container is made of a material selected from magnesium oxide, boron nitride, copper, tungsten, silicon nitride, aluminum nitride, carbon and a combination thereof. The heat treatment of step (iii) can be a single-stage or multi-stage heat treatment.
[0397] Preferably, step (iii) is carried out under an inert gas atmosphere, preferably under an inert gas atmosphere comprising one or more noble gases (such as argon) and / or under a pressure of less than 1 atm, preferably less than 0.1 atm, more preferably less than 0.01 atm. Typically and therefore preferably, step (iii) is carried out under a pressure of less than 10 -4 atm, preferably less than 10 -5 Atm pressure and preferably under an inert gas atmosphere, preferably an inert gas atmosphere comprising one or more noble gases such as argon. In view of potential reactions with the glass precursor, the use of nitrogen as an inert atmosphere should generally be avoided.
[0398] It is highly preferred that the melt-quenching process of the present invention is used to prepare a solid material according to embodiment 1 or embodiment 2 as described herein.
[0399] In some embodiments of the melt quenching method of the present invention, step (iv) further comprises the following steps:
[0400] (iv) a quenching the melt obtained in step (iii) to obtain a solid material;
[0401] (iv) b comminuting the solid material of step (iv) a to obtain a particulate solid, such as a powder; and
[0402] (iv) c optionally forming a film or sheet, preferably a film or sheet having a thickness of less than 500 microns, preferably less than 100 microns, by the following steps:
[0403] - dissolving or suspending the particulate solid of step (iv)b in a liquid phase to obtain a solution or suspension, followed by deposition from the solution or suspension to obtain a film or sheet; or
[0404] - reheating the particulate solid of step (iv)b to a temperature sufficient to allow the film or sheet to be stretched, and stretching the film or sheet.
[0405] In an alternative embodiment, step (iv) comprises quenching the melt of step (iii) while maintaining a sufficiently high temperature to allow stretching of the film or sheet, and stretching the film or sheet, preferably stretching the film or sheet to a thickness of less than 500 microns, preferably less than 100 microns.
[0406] Preferably, the method is operated as a continuous process to produce a continuous glass film or sheet that is cut to desired dimensions.
[0407] The quenching step in step (iv) is preferably performed by directly contacting the melt obtained in step (iii) or contacting the container when closed or open (preferably when closed) with water, ice, an optionally cooled gas (such as air), an optionally cooled metal plate (such as via roller quenching) and / or a chemically inert mold.
[0408] Implementation 4
[0409] In another aspect of the present invention, a solid composition is provided, the solid composition comprising a first solid material, the first solid material being a solid material as described herein (i.e., the solid material of Embodiment 1 or 2), and further comprising at least a second solid material, the second solid material having a composition different from the first solid material. The first solid material may be present in the form of discrete particles embedded in a matrix of the second solid material. Alternatively, the first solid material and the second solid material may be present in the form of discrete particles that have been blended, optionally in combination with a binder material and one or more other materials, and wherein the blend is preferably compacted. Alternatively, the first solid material and the second solid material may be present in the form of different layers of a multilayer sheet or film, preferably with a total thickness of less than 500 microns, preferably less than 200 microns of a multilayer sheet or film. Such solid compositions comprising a first solid material (which is a solid material as described herein) and further comprising at least one second solid material having a different composition from the first solid material are particularly useful as cathodes, anodes or separators of electrochemical cells, particularly as separators or cathodes. In some embodiments, the second solid material is a cathode material, such as a nickel-cobalt or nickel-manganese-cobalt cathode material.
[0410] Implementation 5
[0411] In another aspect of the present invention, an electrochemical cell is provided, the electrochemical cell comprising a solid material as described herein (i.e., the solid material of Embodiment 1 or 2). In particular, an electrochemical cell is provided, wherein the cathode, anode and / or separator comprise a solid material as defined herein. In some embodiments, an electrochemical cell is provided, wherein the cathode, anode and / or separator comprise a solid material as defined herein in the form of a solid composition, the solid composition comprising a first solid material (which is a solid material as described herein), and further comprising at least one second solid material having a different composition from the first solid material. Such solid compositions are described in the context of another aspect of the present invention. In a particularly preferred embodiment of the present invention, an electrochemical cell is provided, wherein the separator comprises a solid material as defined herein, optionally in the form of a solid composition as described herein. In some embodiments, the separator consists of a solid material as described herein.
[0412] Implementation 6
[0413] In another aspect of the present invention, there is provided a use of a solid material as described herein (i.e., the solid material of Embodiment 1 or 2) or a solid composition as described herein (i.e., the solid composition of Embodiment 4) as a solid electrolyte for an electrochemical cell. Preferably, there is provided a use of a solid material as described herein as a solid electrolyte for an electrochemical cell.
[0414] In the context of the various aspects of the invention described herein, suitable electrochemically active cathode materials and suitable electrochemically active anode materials are those known in the art. For example, the anode may comprise graphite carbon, metallic lithium or a metal alloy comprising lithium as an anode active material. For example, the cathode may comprise a nickel-cobalt or nickel-manganese-cobalt cathode material. The electrochemical cell as described herein is preferably a lithium-ion containing cell, wherein charge transport is controlled by Li + Ion impact. The electrochemical cell may have a disc or prismatic shape. The electrochemical cell may include a housing that may be made of steel or aluminum. Multiple electrochemical cells may be combined into an all-solid-state battery having both solid electrodes and solid electrolytes.
[0415] Implementation Plan 7
[0416] Another aspect of the present invention relates to a battery, more specifically a lithium ion battery or a lithium metal battery, comprising at least one electrochemical cell comprising a solid material as described herein (i.e., a solid material of Embodiment 1 or 2), such as two or more electrochemical cells as described in Embodiment 5. Certain embodiments relate to solid-state batteries, preferably lithium solid-state batteries, comprising at least one electrochemical cell comprising a solid material as described herein (i.e., a solid material of Embodiment 1 or 2), such as two or more electrochemical cells as described in Embodiment 5. The electrochemical cells as described in Embodiment 5 can be combined with each other, such as connected in series or in parallel. Series connection is preferred. The electrochemical cells or batteries described herein can be used to manufacture or operate automobiles, computers, personal digital assistants, mobile phones, watches, camcorders, digital cameras, thermometers, calculators, laptop BIOS, communication equipment or remote car locks, as well as fixed applications, such as energy storage devices for power plants.
[0417] Implementation 8
[0418] Another aspect of the invention is a method of manufacturing or operating an automobile, a computer, a personal digital assistant, a mobile phone, a watch, a camcorder, a digital camera, a thermometer, a calculator, a laptop BIOS, a communication device, a remote car lock, and a stationary application (such as an energy storage device for a power plant) by using at least one battery or at least one electrochemical cell comprising a solid material as described herein (i.e., an electrochemical cell as described in Embodiment 5).
[0419] Implementation Plan 9
[0420] Another aspect of the present disclosure is the use of an electrochemical cell comprising the solid material of the present invention (i.e., an electrochemical cell as described in Embodiment 5) in a motor vehicle, a bicycle operated by an electric motor, a robot, an aircraft (e.g., an unmanned aerial vehicle including a drone), a ship, or a stationary energy storage device. The present invention further provides a device comprising at least one electrochemical cell as described in Embodiment 5. Mobile devices, such as vehicles, e.g., cars, bicycles, airplanes, or water vehicles, such as ships or boats, are preferred. Other examples of mobile devices are those portable devices, such as computers, especially laptops, telephones, or power tools, such as from the construction sector, such as drills, battery-driven screwdrivers, or battery-driven nailers.
[0421] Implementation 10
[0422] In another aspect of the present invention, a lithium salt of formula LiX is provided for improving the thermal stability ΔT of a glassy solid. x, especially for improving the thermal stability ΔT of sulfide-based lithium-ion conducting solid electrolytes x Use of, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof, preferably X represents Cl, Br, I or a combination thereof. In some embodiments, there is provided a method for improving the thermal stability ΔT of the glassy solid according to the general formula (II) described in embodiment 2 x The general formula (II), in particular the preferred embodiments of x, y and z described herein in the context of embodiment 2, are equally applicable to the use of embodiment 10.
[0423] The present invention is further illustrated by the following non-limiting examples.
[0424] Example
[0425] 1. Preparation of Materials
[0426] For each example, the following starting products were used to produce 15 g of the final material: amorphous B2S3 (99 wt. %), Li2S (99.9 wt. %), B2O3 (99.95 wt. %) and LiX (LiI (99 wt. %), LiBr (99 wt. %), LiCl (99 wt. %). In an argon-filled glove box, the appropriate amounts of starting materials were weighed, mixed and introduced into a carbon-coated silica ampoule. The tube was sealed and introduced into a vertical shaking furnace. The melt was homogenized at an internal temperature of 950° C. for 30 minutes and then quenched in water at room temperature. The ampoule was then opened in an argon-filled glove box. An orange or brown glassy material with good transparency was obtained.
[0427] For some embodiments, an alternative synthesis was performed with success wherein the amounts of boron and sulfur provided by B2S3 were provided in the form of amorphous elemental B (99 wt %) and elemental S (99.999 wt %).
[0428] 2. Thermal stability ΔT x Determination of
[0429] Thermal analysis was performed using a differential scanning calorimeter DSC 3500 Sirius. Samples of 5 to 10 mg of the glassy material were placed in sealed aluminum pans and analyzed using the following temperature profile: from 100°C to 350°C at a rate of 10°C / min. For each sample, the glass transition temperature (T g ) and crystallization start time (T x ). Then the simple difference between these values (ΔT x = T x – T g ) to estimate thermal stability.
[0430] Glass transition temperature (T g ) is determined by constructing tangents to the baseline of the DSC curve before and after the glass transition and determining the extrapolated onset temperature by the intersection of these tangents, which corresponds essentially to the temperature at which the highest slope of the DSC baseline decrease occurs before the exothermic crystallization peak. The T determined in this way is g The starting temperature is used as T g .
[0431] 3. Determination of conductivity
[0432] The ionic conductivity was measured by electrochemical impedance spectroscopy (EIS) at room temperature (25 °C) on hot pressed samples in particle cells with ion-blocked electrodes. The samples were densified at 350 MPa at 125 °C for 5 min. The ionic conductivity was measured at an operating pressure of 125 MPa. For EIS, an excitation voltage of 10 mV was applied in the frequency range of 7 MHz to 1 Hz. The data were interpreted by equivalent circuit analysis.
[0433] Electronic conductivity was measured on hot pressed samples in particle cells with ion-blocked electrodes at room temperature (25°C). The samples were densified at 350 MPa at 125°C for 5 min. Electronic conductivity was measured at an operating pressure of 125 MPa. Electronic conductivity was measured via stepwise potentiostatic polarization at 0.2 V, 0.4 V and 0.6 V for 20 min.
[0434] Both measurements were performed with a potentiostat with a frequency analyzer (Biologic).
[0435] 4. Determination of properties of the obtained glass
[0436] Inductively coupled plasma optical emission spectroscopy (ICP-OES) was applied to the glassy materials of the examples prepared as explained above.
[0437] A sample of the glassy material was weighed in a glove box under an Ar atmosphere to avoid reaction with water or O2 and added to a microwave vessel. The combination of acids was added, the vessel was closed and digested in the microwave until clear. The matrix elements (Li and B) were analyzed using a high-precision ICP-OES method.
[0438] S was determined via elemental analysis after sample preparation in an Ar-filled glove box. Sample preparation involved inserting about 100 mg of sample into a sealable capsule, followed by adding the sealed capsule and additives to a ceramic crucible. The filled crucible was then heated in an induction furnace under an O2 atmosphere. The S present was released from the sample, converted into SO2 gas and detected by a SO2-specific IR detector. The detected SO2 signal was ultimately converted into S concentration by using a calibration line and taking into account the exact sample mass.
[0439] The composition of the glass was found to correspond, within the expected range of experimental error and variation, to the expected overall formula based on the molar ratios of the precursors subjected to melt quenching.
[0440] 5. Results
[0441]
[0442] Table 1: General formula of synthetic compositions with component A and component B.
[0443]
[0444]
[0445] Table 3: T of Examples 1 to 12 x 、T g , ionic conductivity, and electronic conductivity; NA = not available.
[0446]
[0447] Table 3: (Continued) T of Examples 13 to 20 x 、T g , ionic conductivity and electronic conductivity.
Claims
1. A solid material having a composition according to general formula (I): Li 2c+d B 2a+2b S 3a+c Oh 3b X d (I) in X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof; a is in the range of 0.03 to 0.1; b is in the range of 0 to 0.04; c is in the range of 0.12 to 0.26; and d is in the range of 0.001 to 0.
14.
2. The solid material according to claim 1, wherein X represents Cl, Br, I or a combination thereof.
3. The solid material according to claim 1, wherein a is in the range of 0.06 to 0.1; b is in the range of 0.002 to 0.02; c is in the range of 0.14 to 0.19; and d is in the range of 0.001 to 0.
14.
4. A solid material according to any one of the preceding claims, wherein d is in the range of 0.005 to 0.08, preferably in the range of 0.01 to 0.06, more preferably in the range of 0.01 to 0.
04.
5. A solid material according to any one of the preceding claims, wherein the solid material conforms to formula (I)a, formula (I)b, formula (I)c or formula (I)d: 。 6. A solid material according to any one of the preceding claims, wherein 5a+5b+3c+2d=1.
7. A solid material, preferably a solid material according to any one of the preceding claims, obtainable by melt quenching a mixture of A and B, wherein the molar ratio of A to B in the mixture before quenching is in the range of 60:40 to 99:1; Wherein component A conforms to the general formula (II) xLi2S-yB2S3-zB2O3(II) in x is in the range of 55 to 85, preferably in the range of 55 to 75, more preferably in the range of 60 to 70; y is in the range of 15 to 45, preferably in the range of 20 to 40, more preferably in the range of 25 to 35; z is in the range of 0 to 15, preferably in the range of 0 to 10, more preferably in the range of 0 to 6; x+y+z = 100; and Wherein component B is LiX, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof.
8. The solid material according to claim 7, wherein X represents Cl, Br, I or a combination thereof.
9. The solid material according to claim 7 or 8, wherein x is in the range of 62 to 68, preferably in the range of 63 to 67, more preferably in the range of 64 to 66; y is in the range of 27 to 33, preferably in the range of 28 to 32, more preferably in the range of 29 to 31; z is in the range of 1 to 8, preferably in the range of 3 to 7, more preferably in the range of 4 to 6; and x+y+z = 100.
10. The solid material according to any one of claims 7 to 9, wherein the molar ratio of A to B in the mixture before quenching is in the range of 70:30 to 96:
4.
11. The solid material according to any one of the preceding claims, wherein X represents Br, I or a combination thereof.
12. A solid material according to any one of the preceding claims, wherein the material is a glassy solid.
13. A solid material according to any one of the preceding claims, wherein the material has an ionic conductivity of at least 0.1 mS / cm, preferably at least 0.3 mS / cm at 25°C, and a thermal stability ΔT greater than 100°C, preferably greater than 110°C, more preferably greater than 115°C. x , where ΔT x = T x – T g , where T x is the crystallization onset temperature determined by DSC, and T g is the glass transition temperature determined by DSC.
14. A method for preparing a solid material, preferably a solid material according to any one of claims 1 to 13, the method comprising the steps of: (i) providing the following precursors: •Li2S; • B2S3 and / or both boron and sulfur; • Optionally B2O3; and •LiX, wherein X represents F, Cl, Br, I, N3, SCN, CN, OCN, BF4, BH4 or a combination thereof; (ii) preparing a mixture comprising the precursor provided in step (i), wherein • in said mixture, the molar ratios of the elements Li, S, B, O and X correspond to the general formula (I) as claimed in claims 1 to 6; or • in said mixture, the molar ratio of said precursors complies with the general formula (II) as described in claims 7 to 10, and in said mixture, the molar ratio of A to B is as described in claims 7 to 10; (iii) heat treating the mixture prepared in step (ii) to obtain a melt; as well as (iv) quenching the melt obtained in step (iii) to obtain the solid material, preferably the solid material according to any one of claims 1 to 13.
15. The method of claim 14, wherein X represents Cl, Br, I or a combination thereof.
16. An electrochemical cell comprising the solid material according to any one of claims 1 to 13.
17. The electrochemical cell of claim 16, wherein the separator comprises a solid material according to any one of claims 1 to 13.
18. Use of a solid material according to any one of claims 1 to 13 as a solid electrolyte for an electrochemical cell.
Citation Information
Patent Citations
Sulfide solid electrolyte material, lithium solid battery, and producing method for sulfide solid electrolyte material
CN107134589A
Vitreous solid electrolyte sheets of li ion conducting sulfur-based glass and associated structures, cells and methods
CN107258031A
Sulfide solid electrolyte and preparation and application thereof
CN114361580A
Lithium-ion conducting haloboro-oxysulfides
WO2020254314A1