Multifunctional-layer lithium manganate positive electrode material, preparation method thereof, positive electrode plate and battery

By building a multifunctional layer structure on lithium manganate, combining phase doping, sublayer modification and surface-induced layer, the problems of Mn dissolution and structural stability in high-temperature cycle are solved, and the high-temperature cycle performance of lithium manganate is achieved and Improved storage performance.

CN119008931AInactive Publication Date: 2024-11-22XIANGTAN ELECTROCHEMICAL SCI CO LTD

Patent Information

Application Number
CN202411502564.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium manganate faces the Mn dissolution problem caused by electrolyte corrosion during high-temperature cycle, and a single improvement measure cannot fundamentally solve the problems of structural stability and high-temperature performance.

Method used

Using a multifunctional layer structure, including bulk-doped lithium manganate body, sub-layer doped modified layer and surface-doped crystal surface-induced layer, combined with the surface cladding layer, through the synergy between doping elements and covering elements, Improve structural stability and Li+ diffusion kinetics.

Benefits of technology

It significantly improves the structural stability and high-temperature cycling performance of lithium manganate, inhibits irreversible phase change, improves Mn dissolution, and enhances storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008931A_ABST
    Figure CN119008931A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of energy materials, and provides a multifunctional-layer lithium manganate positive electrode material and a preparation method thereof, a positive electrode plate and a battery, the multifunctional-layer lithium manganate positive electrode material comprises a core body and a surface coating layer, the core body sequentially comprises a bulk phase doped lithium manganate body, a sub-layer doped modification layer and a surface doped crystal face induction layer from an inner core to an outer layer, the chemical formula of the core body is Li < 1 + a > Mn < 2-b-c-d > M N < c > X < d > O < 4-e > Z < e >, and M, N, X and Z are doping elements; the surface coating layer is a compound containing a coating element M ', so that the structural stability of the lithium manganate can be remarkably improved, irreversible phase change of the lithium manganate in the cycle process is inhibited, Mn dissolution at high temperature is improved, the structural stability and Li < + > diffusion kinetics are improved, and the high-temperature cycle performance of the lithium manganate is further improved; the lithium ion secondary battery prepared from the positive electrode material has relatively high initial specific discharge capacity and excellent high-temperature cycle and high-temperature storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of energy materials, and in particular relates to a multifunctional layer lithium manganese oxide positive electrode material and a preparation method thereof, a positive electrode plate and a battery. Background Art

[0002] At present, the mainstream positive electrode materials of lithium-ion batteries include lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and nickel cobalt manganese oxide. Among them, lithium manganese oxide (LiMn2O4) has become a lithium-ion positive electrode material with great application prospects due to its advantages such as low cost, high rate and high safety. However, lithium manganese oxide faces serious challenges such as Jahn-Teller effect, manganese dissolution and irreversible phase change during the cycle process. In order to overcome these problems, people have adopted various strategies, such as bulk doping and surface coating. Among them, doping elements such as Ni, Co, Ti, Zr, Mg, Al, F, B, S can improve the structural stability of lithium manganese oxide and improve the performance of lithium manganese oxide, but the problem of Mn dissolution caused by the corrosion of the electrolyte at high temperature has not been fundamentally solved. In order to improve the high-temperature cycle performance of lithium manganese oxide, a surface coating strategy is often used to avoid direct contact between the electrolyte and the active material, thereby slowing down the corrosion of the positive electrode material and Mn dissolution at high temperature and improving the high-temperature performance of lithium manganese oxide. However, these coating materials are not conducive to the interaction between electrons and Li + The transmission dynamics of lithium manganese oxide are affected, and the lattice strain during the cycle causes phase separation, thereby reducing the capacity retention rate of the battery. A single improvement measure cannot fundamentally solve the existing problems of lithium manganese oxide. In order to comprehensively improve the structural stability, high-temperature cycle performance and storage performance of lithium manganese oxide, lithium manganese oxide must be improved from the inside out, comprehensively and systematically. Summary of the invention

[0003] The embodiments of the present application provide a multifunctional layer lithium manganese oxide positive electrode material and a preparation method thereof, a positive electrode plate and a battery, which aim to solve the problem of Mn dissolution caused by electrolyte corrosion at high temperature in the lithium manganese oxide positive electrode material to a certain extent, and improve the structural stability, high temperature cycle performance and storage performance of lithium manganese oxide.

[0004] In order to solve the above technical problems, the technical solution proposed by the present invention is: In the first aspect, a multifunctional layered lithium manganese oxide positive electrode material is provided, comprising a core body and a surface coating layer, wherein the core body is composed of a bulk-doped lithium manganese oxide body, a sub-layer doped modification layer and a surface-doped crystal surface induction layer from the inner core to the outer layer, and the chemical formula of the core body is Li 1+a Mn 2-b-c-d M b R c X d O 4-e Z e, wherein M, R, X, and Z are doping elements; the surface coating layer is a compound containing the coating element M', wherein -0.1≤a≤0.3, 0≤b≤0.3, 0≤c≤0.3, 0≤d≤0.3, and 0≤e≤0.3, and at least one of b, c, d, and e is not 0; the total mass ratio of the coating element in the surface coating layer to the total mass of the core doping element is 1:(0.5-10).

[0005] The present application provides a multifunctional layered lithium manganese oxide positive electrode material, which can significantly improve the structural stability of lithium manganese oxide, inhibit the irreversible phase change during the lithium manganese oxide cycle, improve the Mn dissolution at high temperature, and improve the structural stability and Li + Diffusion kinetics, thereby improving the high temperature cycling performance of lithium manganese oxide.

[0006] In a second aspect, a method for preparing the multifunctional layer lithium manganese oxide positive electrode material according to the first aspect is provided, comprising: S1, mixing a manganese-containing compound into a dopant containing an M element through a doping process, uniformly mixing the mixture through different processes to obtain a positive electrode active material precursor, and then mixing the positive electrode active material precursor with a dopant containing R, X, and Z elements and a lithium salt, and then performing a first sintering to obtain a lithium manganate positive electrode material core; S2, coating the inner core of the lithium manganate positive electrode material obtained in S1 with a coating material containing the M' element, and obtaining a multifunctional layer lithium manganate positive electrode material after a second sintering.

[0007] In a third aspect, a positive electrode plate is provided, comprising a current collector and a positive electrode active material layer arranged on at least one surface of the current collector, the positive electrode plate adopts the multifunctional layer lithium manganese oxide positive electrode material described in the first aspect, or the multifunctional layer lithium manganese oxide positive electrode material prepared by the preparation method described in the second aspect.

[0008] Due to the use of multifunctional layered lithium manganate positive electrode material, the positive electrode plate of the present invention can enable the lithium-ion secondary battery to have excellent structural stability, high-temperature cycle performance and storage performance at the same time.

[0009] In a fourth aspect, a lithium-ion secondary battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet is the positive electrode sheet described in the third aspect of the present invention.

[0010] Due to the use of the multifunctional layer lithium manganate positive electrode material of the first aspect of the embodiment of the present invention, the lithium ion secondary battery can simultaneously have excellent structural stability, high temperature cycle performance and storage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0012] Figure 1 It is a schematic diagram of a multifunctional layer-modified lithium manganese oxide positive electrode material; Figure 2 This is the XRD diagram of the multifunctional layer lithium manganese oxide positive electrode material prepared by the present invention; Figure 3 SEM image of the multifunctional layer modified lithium manganese oxide positive electrode material prepared by the present invention. DETAILED DESCRIPTION

[0013] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0014] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0015] In the present application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.

[0016] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. For example, without departing from the scope of the implementation regulations of this application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0017] The terms used in the embodiments of the present application are only for the purpose of describing specific implementation rules, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the implementation rules of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0018] It should be understood that in the various embodiments of the present application, the size of the serial number of each process does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the implementation regulations of this application.

[0019] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0020] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0021] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0022] The technical solution of the present application is illustrated below through specific embodiments and comparative examples.

[0023] A multifunctional layered lithium manganese oxide positive electrode material comprises a core body and a surface coating layer, wherein the core body is composed of a bulk phase doped lithium manganese oxide body, a sub-layer doped modification layer and a surface doped crystal surface induction layer from the inner core to the outer layer, and the chemical formula of the core body is Li 1+a Mn 2-b-c-d M b R c X d O 4-e Z e , wherein M, R, X, and Z are doping elements; the surface coating layer is a compound containing the coating element M', wherein -0.1≤a≤0.3, 0≤b≤0.3, 0≤c≤0.3, 0≤d≤0.3, and 0≤e≤0.3, and at least one of b, c, d, and e is not 0; the total mass ratio of the coating element in the surface coating layer to the total mass of the core doping element is 1:(0.5-10).

[0024] In one embodiment, the bulk-doped lithium manganese oxide body doping elements are M and Z, wherein M is a doping element of a metal manganese site of the lithium manganese oxide body, and M is selected from one or more of Ni, Sn, Y, Co, Si, Cu, Zn, Ca, Fe, V, Al, Zr, Ti, Mg, La, Ga, In and Ge, and Z is a doping element of an oxygen site of the lithium manganese oxide body, and Z is selected from one or more of N, F, Cl, Br, I, P, B and S, and the mass concentration deviation of the M and Z elements at any point in the lithium manganese oxide body is less than 20%; The doping element of the sub-layer modification layer is R, and R is the doping element doped in the metal manganese site in the sub-layer doping modification layer, and R is selected from one or more of Sn, Mg, La, Co, Mo, Zr, Yb, Al, Ni, Ti, Nb, V, Y, Ru, Sr, Al, In and Ba; The doping element of the surface doped crystal plane inducing layer is X, and X is the doping element in the surface doped crystal plane inducing layer, and X is selected from one or more of Y, Al, W, Ni, La, Ba, Zr, Ti, Sn, Nb, V, Ce, Co, Cu, Mg, Sr, In, Yb, Mo, Ru and Ta.

[0025] In one embodiment, the surface coating layer is one or a combination of oxides, fluorides, phosphates, carbonates, sulfates, nitrates, chlorides, acetates, lithium-ion battery positive electrode materials or conductive organic substances containing a coating element M', wherein M' is selected from a combination of one or more of B, Mg, La, Nb, Co, Ta, Al, Yb, Zr, Li, Sr, Ti, Ce, Ni, Y, Sn, Ru, V, In, Cu, Mn, Mo and W, and the conductive organic substance is PAIN, PEG, PPy, PEDOT, or PSS.

[0026] In one embodiment, the chemical formula of the lithium-ion battery positive electrode material includes Li 1+i (TM) x PO4 and / or Li 1+i (TM) x O2, wherein TM is one or more transition metal elements, wherein 0≤i≤0.3, 0≤x≤1.

[0027] In one embodiment, when the average particle size of the multifunctional layer lithium manganese oxide positive electrode material is ≤ 1 / 5 of the thickness of the multifunctional layer lithium manganese oxide positive electrode material along the surface coating layer toward the inner core, the mass ratio of the sum of the mass of the doping element and the coating element to the sum of the mass of the doping element and the coating element in the multifunctional layer lithium manganese oxide positive electrode material is 45% to 99%.

[0028] When the outer surface of the lithium manganese oxide positive electrode material is at 1 / 2 of the inner diameter, the mass content ratio of the sub-layer doping to the bulk doping element is 1:1 to 20, preferably 1:10. When the outer surface of the lithium manganese oxide positive electrode material is at 1 / 2 of the inner core, the mass content ratio of the element of the crystal plane induction layer to the bulk doping element is 1:6, preferably 1:3.

[0029] In one embodiment, when the average particle size of the multifunctional layer lithium manganese oxide positive electrode material is ≤ 2 / 3 of the multifunctional layer lithium manganese oxide positive electrode material along the surface coating layer toward the inner core, the mass ratio of the sum of the mass of the doping element and the coating element to the sum of the mass of the doping element and the coating element in the multifunctional layer lithium manganese oxide positive electrode material is 90% to 99%.

[0030] The discharge capacity, cycle performance and storage performance of spinel lithium manganese oxide positive electrode materials are closely related to the physical and chemical properties of the material itself. In the structure of lithium manganese oxide positive electrode materials, Mn is the main active metal component, and its average valence is +3.5. + In the process, it is oxidized to Mn 4+ , so in lithium-ion secondary batteries, Li + In the process of lithium manganese oxide, the charge balance is mainly achieved by the change of the valence state of Mn. 3+ Prone to disproportionation reaction to generate Mn 4+ and soluble Mn 2+ , Mn 2+ It is easy to dissolve in the electrolyte, resulting in the loss of active Mn, causing capacity decay and shortening the cycle life of lithium manganese oxide batteries. This dissolution phenomenon is more significant at high temperatures. 3+ The Jahn-Teller reaction during the charge and discharge process affects the structural stability of lithium manganese oxide, which is not conducive to the long-term cycle of lithium manganese oxide. The spinel structure of lithium manganese oxide exposes the (111) crystal plane that is prone to disproportionation reaction and Mn dissolution, further deteriorating the battery performance. The large specific surface area also easily aggravates the corrosion of HF decomposed by the electrolyte to lithium manganese oxide. 4+ content, reducing Mn 3+ content and enhance the structural stability of lithium manganese oxide, but a single doping strategy still cannot solve the problems existing in lithium manganese oxide.

[0031] Therefore, the present application adopts a multifunctional layer of lithium manganese oxide positive electrode material, and each layer cooperates with each other to solve the above problems.

[0032] Based on the general inventive concept, the present invention also provides a method for preparing a multifunctional layer lithium manganese oxide positive electrode material, comprising: S1, doping a manganese-containing compound with a dopant containing an M element through a doping process, uniformly mixing the dopant to obtain a positive electrode active material precursor, and then mixing the positive electrode active material precursor with a dopant containing R, X, and Z elements and a lithium salt, and then performing a first sintering to obtain a lithium manganate positive electrode material core; S2, coating the inner core of the lithium manganate positive electrode material obtained in S1 with a coating material containing the M' element, and obtaining a multifunctional layer lithium manganate positive electrode material after a second sintering.

[0033] In one embodiment, the manganese-containing compound in S1 is a combination of one or more of Mn3O4, MnO2 and Mn2O3; the doping process is solid phase doping or liquid phase doping; the lithium salt is a combination of one or more of lithium hydroxide, lithium carbonate and lithium nitrate; the coating in S2 adopts solid phase coating or liquid phase coating; the first sintering conditions in S1 are: in air or oxygen atmosphere, the heating rate is 1-5°C / min, the sintering temperature is 700-900°C, and the sintering time is 12-30h, and the second sintering conditions in S2 are: in air or oxygen atmosphere, the heating rate is 1-5°C / min, the sintering temperature is 300-750°C, and the sintering time is 6-24h.

[0034] Solid phase doping includes: one or more of ball milling, high mixing or oblique mixing; Liquid phase doping includes: one or more of sol-gel method, hydrothermal method, coprecipitation method or spray drying method; Solid phase coating includes one or more of ball milling, high mixing or oblique mixing; Liquid phase coating includes one or more of sol-gel method, hydrothermal method, co-precipitation method or spray drying method.

[0035] The preparation process of this scheme utilizes the different valence states, atomic radii and binding energies with oxygen of each element, and presents a multifunctional layer distribution in the lithium manganese oxide body after high-temperature sintering. Some elements with small atomic radii are easy to diffuse into the lithium manganese oxide body to form a bulk doping structure, while some elements with crystal plane induction function induce the growth of the lithium manganese oxide crystal plane, thereby forming a crystal plane induction layer. Sublayer modification elements, due to their own atomic radius and different binding energies with oxygen, mostly remain on the lithium manganese oxide subsurface, and modify the sublayer structure of lithium manganese oxide. After modification of the above functional layers, the lithium manganese oxide will have more excellent high-temperature performance.

[0036] Based on the general inventive concept, the present invention also provides a positive electrode plate, comprising a current collector and a positive electrode active material layer arranged on at least one surface of the current collector, wherein the positive electrode active material layer comprises the above-mentioned multifunctional layer lithium manganese oxide positive electrode material and the multifunctional layer lithium manganese oxide positive electrode material obtained by the above-mentioned preparation method.

[0037] Specifically, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector includes two opposite surfaces in its thickness direction, and the positive electrode active material layer is stacked on any one or both of the two surfaces of the positive electrode current collector.

[0038] In addition, the positive electrode active material layer may also include a conductive agent and a binder. The present invention does not specifically limit the types of the conductive agent and the binder in the positive electrode active material layer, and they can be selected according to actual needs.

[0039] For example, the conductive agent can be one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers; the binder can be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylic resin and polyvinyl alcohol (PVA).

[0040] The positive electrode current collector may be a metal foil or porous metal plate with good electrical conductivity and mechanical properties, and its material may be one or more of aluminum, copper, nickel, titanium, silver and their respective alloys. The positive electrode current collector is, for example, aluminum foil.

[0041] The positive electrode sheet can be prepared according to conventional methods in the art. For example, the multifunctional layer lithium manganese oxide positive electrode material, the conductive agent and the binder are dispersed in a solvent, and the solvent can be N-methylpyrrolidone (NMP) to form a uniform positive electrode slurry, and the positive electrode slurry is coated on the positive electrode current collector, and after drying, rolling and other processes, the positive electrode sheet is obtained.

[0042] Based on the general inventive concept, the present invention also provides a lithium-ion secondary battery, comprising the above-mentioned positive electrode plate.

[0043] The negative electrode plate may be a metal lithium plate, or may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector.

[0044] The negative electrode active material layer includes a negative electrode active material. The negative electrode active material can be natural graphite, artificial graphite, soft carbon, silicon, silicon-carbon composite, SiO m (0<m<2, such as m=1), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate Li4Ti5O 12, Li-Al alloy and one or more of metallic lithium.

[0045] The negative electrode active material layer may further include a conductive agent and a binder. The conductive agent is one or more of graphite, acetylene black, carbon black, Ketjen black, carbon nanotubes, and graphene; the binder is one or more of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, and carboxymethyl cellulose (CMC).

[0046] The negative active material layer may also optionally include a thickener, such as carboxymethyl cellulose (CMC).

[0047] The negative electrode current collector may be a metal foil or a porous metal plate with good electrical conductivity and mechanical properties, and its material may be one or more of copper, nickel, titanium, iron and their respective alloys. The negative electrode current collector is, for example, copper foil.

[0048] The negative electrode sheet can be prepared according to conventional methods in the art. For example, the negative electrode active material, conductive agent, binder and thickener are dispersed in a solvent, and the solvent can be N-methylpyrrolidone (NMP) or deionized water to form a uniform negative electrode slurry, and the negative electrode slurry is coated on the negative electrode current collector, and after drying, rolling and other processes, the negative electrode sheet is obtained.

[0049] In the lithium-ion secondary battery of the embodiment of the invention, the electrolyte may be a solid electrolyte, such as a polymer electrolyte, an inorganic solid electrolyte, etc., but is not limited thereto. The electrolyte may also be an electrolyte. The electrolyte includes a solvent and a lithium salt dissolved in the solvent.

[0050] The solvent may be ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), preferably two or more thereof.

[0051] The lithium salt may be one or more of LiPF6 (lithium hexafluorophosphate), LiClO4 (lithium perchlorate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), and LiTFS (lithium trifluoromethanesulfonate).

[0052] The electrolyte may also contain other additives, such as one or more of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), succinonitrile (SN), adiponitrile (ADN), glutaronitrile (GLN), hexanetrinitrile (HTN), dimethyl sulfite (DMS), sulfonate cyclic quaternary ammonium salt, tris(trimethylsilyl) phosphate (TMSP) and tris(trimethylsilyl) borate (TMSB), but are not limited thereto.

[0053] The lithium-ion secondary battery of the embodiment of the present invention has no particular limitation on the separator, and a porous structure separator can be selected, such as a single-layer or multi-layer film of one or more of glass fiber, non-woven fabric, polyethylene (PE), polypropylene (PP) and polyvinylidene fluoride (PVDF).

[0054] The positive electrode sheets and the negative electrode sheets are alternately stacked, and a separator is arranged between the positive electrode sheets and the negative electrode sheets to play an isolating role, to obtain a battery cell, or the battery cell can be obtained by winding. The battery cell is placed in a shell, an electrolyte is injected, and it is sealed to obtain a lithium-ion secondary battery.

[0055] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, and to significantly demonstrate the improved performance of the embodiments of the present application, the above technical solutions are illustrated by means of multiple embodiments below.

[0056] Embodiment 1: Preparation of a multifunctional layer lithium manganese oxide positive electrode material: S1. Preparation of nickel-doped spherical manganese tetraoxide precursor: add 10L pure water as the bottom liquid to a 50L reactor, control the stirring speed to 500r, maintain a constant temperature of 60°C, add 9mol / L ammonia solution to the reactor at a pH of 12. Continue to add manganese sulfate solution and nickel sulfate solution to the reactor to obtain a mixed metal salt solution doped with nickel salt, wherein the molar ratio of the mixed metal salt solution doped with nickel salt to NaOH is maintained at 1:2, and the molar ratio of NaOH solution to ammonia water is 1:1, and the pH in the reactor is maintained at 11, and the slurry is continuously reacted to synthesize a nickel-doped manganese tetraoxide precursor. Then the slurry is washed with deionized water, filtered, and dried at 120°C for 12h to obtain a spherical manganese tetraoxide precursor doped with Ni with a particle size D50 of 7μm.

[0057] Preparation of the inner core of lithium manganate cathode material: lithium hydroxide, spherical manganese tetraoxide precursor, TiO2, W2O3, and LiF are placed in a high-speed mixer for high-speed mixing, and the molar ratio of lithium to manganese is maintained at 0.53. The doping amount of Ti accounts for 1934ppm of the lithium manganate cathode material, the doping amount of W accounts for 3687ppm of the lithium manganate cathode material, and the doping amount of F accounts for 897ppm of the lithium manganate cathode material. The mixed material is placed in a track kiln for sintering, calcined at 800℃ for 12h, and the sintering atmosphere is compressed air. The lithium manganate cathode material with Ni and F bulk doping, Ti sublayer doping modification, and W surface crystal plane induced is obtained as the inner core.

[0058] S2. Preparation of coated lithium manganate positive electrode material: The lithium manganate positive electrode material obtained above, which is doped with Ni and F in bulk phase, modified with Ti sublayer doping, and induced with W surface crystal plane, is added into a high-speed mixer together with Al2O3 powder, wherein the coating amount of Al accounts for 4698ppm of the entire lithium manganate positive electrode material. The mixed powder is mixed at a speed of 800r / min for 20min, and the obtained uniformly mixed powder is annealed at 600°C for 4h in a compressed air calcination atmosphere, thereby obtaining a multifunctional layer lithium manganate positive electrode material with 3941ppm Ni and 897ppm F in bulk phase doping, 1934ppm Ti sublayer doping, 1687ppm W crystal plane induction, and Al2O3 surface coating.

[0059] Figure 1 This is a schematic diagram of the multifunctional layer lithium manganese oxide positive electrode material of this embodiment. The figure shows the element distribution of different functional layers of lithium manganese oxide modified by the multifunctional layer. It can be seen from the figure that the main material has four functional areas. The elements of the bulk doping layer are evenly distributed in the particles, the surface distribution of the crystal plane induction layer elements is higher, and decreases toward the inside of the main body, and the sub-layer modified elements are mainly distributed on the sub-surface of the main body particles to form a surface functional layer. After the above functional layer modification, a surface coating layer is constructed on the surface of the main body particles. The sub-layer modified elements, crystal plane induction elements, and bulk doping elements have overlapping distribution areas on the sub-surface, and the crystal plane induction elements and bulk doping elements also have certain overlapping distribution areas inside the material, but to the center of the main body phase, it is mainly the distribution of bulk doping elements. Bulk doping is distributed in the entire material, and the distribution uniformity is good.

[0060] Embodiments 2 to 15: Different from Example 1, the relevant parameters and substances in the preparation steps of the positive electrode active material are changed to obtain a positive electrode active material with predetermined parameter characteristics.

[0061] The first sintering system of step S1 of embodiments 1 to 3, 6 to 8 and 11 to 13 is sintering at 800° C. for 12 h; The first sintering system of step S1 of embodiments 4-5, 9-10 and 14-15 is sintering at 780° C. for 15 h; The second sintering system of step S2 of Examples 1 to 7, 10 to 12, and 15 is sintering at 600° C. for 6 h; The second sintering system of step S2 of Examples 8-9, 13-14 is sintering at 300° C. for 6 h; The lithium source of Example 7 and Example 11 is lithium carbonate.

[0062] Among them, the positive electrode active material precursor of Examples 2 to 10 is Mn3O4; and the positive electrode active material precursor of Examples 11 to 15 is MnO2.

[0063] Among them, Examples 1 to 5 are liquid phase doped Mn3O4 precursors, Examples 6 to 10 are undoped Mn3O4 precursors, and Examples 11 to 15 are undoped MnO2 precursors.

[0064] The types and contents of doping elements are shown in Table 1.

[0065]

[0066] Comparative Examples 1 to 14: The difference from Example 1 is that the relevant parameters and substances in the preparation steps of the positive electrode active material are changed to obtain a positive electrode active material with predetermined parameter characteristics. Among them, the positive electrode active material precursors of Comparative Examples 1 to 10 are all doped with Mn3O4 by the liquid phase method; the positive electrode active material precursors of Comparative Examples 11 to 12 are all doped with Mn3O4 by the solid phase method; and the positive electrode active material precursors of Comparative Examples 13 to 14 are all MnO2.

[0067] The types and contents of doping elements are shown in Table 2.

[0068]

[0069] Test example: 1. Preparation of button cell The multifunctional layer lithium manganese oxide positive electrode material, conductive carbon black and binder PVDF prepared above are dispersed in a solvent N-methylpyrrolidone (NMP) at a weight ratio of 95:3:2 and mixed evenly to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.

[0070] In a button battery box, the positive electrode sheet, the isolation membrane and the metal lithium sheet are stacked in sequence, and the above-mentioned electrolyte is injected to assemble a button battery.

[0071] 2. Preparation of full battery The positive electrode active material, conductive agent acetylene black and binder PVDF prepared above were dispersed in solvent NMP at a weight ratio of 95:3:2 and mixed evenly to obtain positive electrode slurry; the positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.

[0072] The negative electrode active material artificial graphite, hard carbon, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are dispersed in deionized water at a weight ratio of 90:5:2:2:1 and mixed evenly to obtain a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector aluminum foil, and after drying and cold pressing, a negative electrode sheet is obtained.

[0073] A polypropylene (PP) porous polymer film is used as a separator. The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order to obtain a bare cell, which is then placed in an outer package, injected with the above electrolyte and packaged, and then subjected to formation and other processes to obtain a full battery.

[0074] 3. Test part (1) Initial gram capacity test of button cell At 60℃, charge the battery at a constant current of 0.1C to a charge cut-off voltage of 4.3V, then charge at a constant voltage to a current less than or equal to 0.01C, then jump to the rest step, the battery is left for 2 minutes, and then discharged at a constant current of 0.1C to a discharge cut-off voltage of 3.0V. The discharge capacity at this time is the initial gram capacity of the button battery.

[0075] (2) Initial gram capacity test of full battery At 25°C, charge the battery at a constant current of 0.2C to a charge cut-off voltage of 4.3V, then charge at a constant voltage to a current less than or equal to 0.01C, leave it for 5 minutes, and then discharge it at a constant current of 0.2C to a discharge cut-off voltage of 3.0V. The discharge capacity at this time is the initial gram capacity of the whole battery.

[0076] (3) High temperature cycle performance test of full battery At 60°C, charge the battery at 1C constant current to a charge cut-off voltage of 4.3V, then charge at constant voltage to a current less than or equal to 0.01C, leave for 5 minutes, and then discharge at 1C constant current to a discharge cut-off voltage of 3.0V. This is a charge and discharge cycle, and the discharge capacity of this time is recorded as the discharge specific capacity D1 of the first cycle. Perform 100 cycle charge and discharge tests on the battery according to the above method, and record the discharge specific capacity D100 of the 100th cycle. Full battery at 60°C, 1C / 1C cycle 100 times capacity retention rate (%) = D100 / D1×100%.

[0077] (4) High temperature storage performance test of full battery At 60°C, a soft-pack battery with a designed capacity of 1Ah is charged at a constant current of 1C to 100% SOC state with a cut-off voltage of 4.3V, and then charged at a constant voltage to a current less than or equal to 0.01C. The battery is then placed in a constant temperature box at 60°C and stored for 30 days. It is then discharged at a constant current of 1C to a discharge cut-off voltage of 3.0V, and the battery's discharge specific capacity D2 is recorded. The capacity retention rate of the full battery after 30 days of storage = D2 / 1Ah×100%.

[0078] In tests (1)-(4), in Examples 1-15 and Comparative Examples 1-14, the charge and discharge cut-off voltage of the button cell was 3.0V-4.3V, and the charge and discharge cut-off voltage of the full cell was 3.0V-4.3V; The test data of the button cells and full cells of Examples 1 to 15 and Comparative Examples 1 to 14 are shown in Tables 3 and 4.

[0079] The groups forming the performance comparison are: Example 1 and Comparative Example 1, Example 1 and Comparative Example 6, Example 2 and Comparative Example 2, Comparative Example 7, Example 3 and Comparative Example 3, Example 4 and Comparative Example 4, Comparative Example 8, Example 5 and Comparative Example 5, Comparative Example 9; Example 8 and Comparative Example 11, Example 9 and Comparative Example 12, Example 11 and Comparative Example 13, Example 12 and Comparative Example 14.

[0080] Figure 2 The XRD pattern of the multifunctional layer-modified lithium manganese oxide positive electrode material is shown in the figure. As shown in the figure, the XRD spectrum of the multifunctional layer-modified lithium manganese oxide positive electrode material matches the standard card PDF#70-3120 of lithium manganese oxide; Figure 3 This is a SEM picture of a multifunctional layer-modified lithium manganese oxide positive electrode material. As shown in the figure, the multifunctional layer-modified lithium manganese oxide positive electrode material is composed of primary particles with smooth surfaces, and a single particle has an octahedral structure with blunt edges and corners.

[0081]

[0082]

[0083] Through the comparison results of Examples 1 to 15 and Comparative Examples 1 to 14, it can be seen that by uniform bulk doping of M and Z elements, sublayer modification of N element, crystal plane induction of X element, and then covering the surface of the lithium manganese oxide positive electrode material body particles with a surface coating layer of M', the lithium ion secondary battery can have a higher initial discharge specific capacity and excellent high temperature cycle and high temperature storage performance.

[0084] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0085] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A multifunctional layer lithium manganese oxide positive electrode material, characterized in that: It includes a core body and a surface coating layer, wherein the core body is composed of a bulk-doped lithium manganate body, a sub-layer doped modification layer and a surface-doped crystal surface induction layer from the inner core to the outer layer, and the chemical formula of the core body is Li 1+a Mn 2-b-c-d M b R c X d O 4-e Z e , wherein M, R, X, and Z are doping elements; the surface coating layer is a compound containing the coating element M', wherein -0.1≤a≤0.3, 0≤b≤0.3, 0≤c≤0.3, 0≤d≤0.3, and 0≤e≤0.3, and at least one of b, c, d, and e is not 0; the total mass ratio of the coating element in the surface coating layer to the total mass of the core doping element is 1:(0.5-10).

2. The multifunctional layer lithium manganate positive electrode material according to claim 1, characterized in that: The doping elements of the bulk-doped lithium manganese oxide body are M and Z, wherein M is a doping element of the metal manganese site of the lithium manganese oxide body, and M is selected from one or more of Ni, Sn, Y, Co, Si, Cu, Zn, Ca, Fe, V, Al, Zr, Ti, Mg, La, Ga, In and Ge, and Z is a doping element of the oxygen site of the lithium manganese oxide body, and Z is selected from one or more of N, F, Cl, Br, I, P, B and S, and the mass concentration deviation of the M and Z elements at any point in the lithium manganese oxide body is less than 20%; The doping element of the sub-layer modification layer is R, and R is the doping element doped in the metal manganese site in the sub-layer doping modification layer, and R is selected from one or more of Sn, Mg, La, Co, Mo, Zr, Yb, Al, Ni, Ti, Nb, V, Y, Ru, Sr, Al, In and Ba; The doping element of the surface doped crystal plane inducing layer is X, and X is the doping element in the surface doped crystal plane inducing layer, and X is selected from one or more of Y, Al, W, Ni, La, Ba, Zr, Ti, Sn, Nb, V, Ce, Co, Cu, Mg, Sr, In, Yb, Mo, Ru and Ta.

3. The multifunctional layer lithium manganese oxide positive electrode material according to claim 1, characterized in that: The surface coating layer is one or a combination of oxides, fluorides, phosphates, carbonates, sulfates, nitrates, chlorides, acetates, lithium-ion battery positive electrode materials, and conductive organic substances containing a coating element M', wherein M' is selected from one or a combination of B, Mg, La, Nb, Co, Ta, Al, Yb, Zr, Li, Sr, Ti, Ce, Ni, Y, Sn, Ru, V, In, Cu, Mn, Mo, and W, and the conductive organic substance is PAIN, PEG, PPy, PEDOT, or PSS.

4. The multifunctional layer lithium manganese oxide positive electrode material according to claim 3, characterized in that: The general chemical formula of the positive electrode material of the lithium ion battery includes Li 1+i (TM) x PO4 and / or Li 1+i (TM) x O2, wherein TM is one or more transition metal elements, wherein 0≤i≤0.3, 0≤x≤1.

5. The multifunctional layer lithium manganese oxide positive electrode material according to claim 1, characterized in that: When the average particle size of the multifunctional layer lithium manganese oxide positive electrode material is ≤ 1 / 5 of the thickness of the multifunctional layer lithium manganese oxide positive electrode material along the surface coating layer toward the inner core, the mass ratio of the sum of the mass of the doping element and the coating element to the sum of the mass of the doping element and the coating element in the multifunctional layer lithium manganese oxide positive electrode material is 45% to 99%.

6. The multifunctional layer lithium manganese oxide positive electrode material according to claim 1, characterized in that: When the average particle size of the multifunctional layer lithium manganese oxide positive electrode material is ≤ 2 / 3 of the multifunctional layer lithium manganese oxide positive electrode material along the surface coating layer toward the inner core, the mass ratio of the sum of the mass of the doping element and the coating element to the sum of the mass of the doping element and the coating element in the multifunctional layer lithium manganese oxide positive electrode material is 90% to 99%.

7. A method for preparing a multifunctional layer lithium manganate positive electrode material according to any one of claims 1 to 6, characterized in that: include: S1, mixing a manganese-containing compound into a dopant containing an M element through a doping process, uniformly mixing the mixture, and obtaining a positive electrode active material precursor; then mixing the positive electrode active material precursor with a dopant containing R, X, and Z elements and a lithium salt, and performing a first sintering to obtain a lithium manganate positive electrode material core; S2, coating the inner core of the lithium manganate positive electrode material obtained in S1 with a coating material containing the M' element, and obtaining a multifunctional layer lithium manganate positive electrode material after a second sintering.

8. The preparation method according to claim 7, characterized in that: The manganese-containing compound in S1 is a combination of one or more of Mn3O4, MnO2 and Mn2O3; And / or, the doping process is solid phase doping or liquid phase doping; And / or, the lithium salt is a combination of one or more of lithium hydroxide, lithium carbonate and lithium nitrate; And / or, the coating in S2 is carried out by solid phase coating or liquid phase coating; And / or, the first sintering conditions in S1 are: in air or oxygen atmosphere, the heating rate is 1-5°C / min, the sintering temperature is 700-900°C, and the sintering time is 12-30h; the second sintering conditions in S2 are: in air or oxygen atmosphere, the heating rate is 1-5°C / min, the sintering temperature is 300-750°C, and the sintering time is 6-24h.

9. A positive electrode sheet, characterized in that: It comprises a current collector and a positive electrode active material layer arranged on at least one surface of the current collector, wherein the positive electrode active material layer comprises the multifunctional layer lithium manganate positive electrode material according to any one of claims 1 to 6, or the multifunctional layer lithium manganate positive electrode material obtained by the preparation method according to any one of claims 7 to 8.

10. A lithium ion secondary battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, and the positive electrode sheet is the positive electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Gradient doped type lithium-ion cathode material and method for preparing same

    CN103000878A

  • Positive electrode active material and preparation method thereof, positive electrode plate and lithium ion secondary battery

    CN112447950A

  • Positive electrode active material, preparation method thereof, positive electrode plate and lithium ion secondary battery

    CN112447951A

  • Monocrystal lithium manganate positive electrode material and preparation method thereof

    CN113285068A

  • Positive electrode active material and preparation method thereof, positive electrode and lithium ion secondary battery

    CN114512642A

Cited By

  • Positive electrode active material and preparation method thereof, positive plate and battery

    CN119542395A

  • Preparation method of positive active material, positive active material, positive plate and battery

    CN119542396A

  • Lithium ion battery positive electrode material, preparation method thereof and lithium ion battery

    CN120033234A

  • A lithium ion battery positive electrode material and preparation method thereof and lithium ion battery

    CN120033234B

  • Multifunctional-layer lithium manganate positive electrode material, preparation method thereof and lithium battery

    CN120998990A