Method for simply preparing ceramic membrane with small pore diameter, narrow pore diameter distribution and high pollution resistance and product

The ceramic membrane was prepared by scraping coating, and the problems of wide pore size distribution and poor anti-pollution performance of the ceramic membrane were solved, small pore size distribution and high-efficiency oil-water separation were achieved, simplifying the preparation process and reducing the sintering temperature.

CN119015900AActive Publication Date: 2024-11-26TIANJIN POLYTECHNIC UNIV

Patent Information

Application Number
CN202411397018.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-26
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

The existing ceramic membrane has a wide pore size distribution and poor anti-pollution performance in oil-water separation, and the preparation process is complicated, making it difficult to achieve small pore size and efficient separation.

Method used

The ceramic film was prepared by scraping coating method, and a commercial ceramic film with an average pore diameter of 300-500nm was used as the base film, and ceramic particles, inorganic binders, water-soluble polymers and surfactants were added to form 50-100nm by sintering. The ceramic membrane is distributed with a narrow pore size to improve the anti-pollution ability.

Benefits of technology

The simple preparation of small-pore and narrow-pore distribution ceramic membranes is achieved, which significantly improves the separation performance and oil pollution resistance of small-sized emulsified oil wastewater, simplifies the preparation process, and reduces the sintering temperature.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance and a product, and belongs to the technical field of ceramic membrane separation. Specifically, a commercial ceramic membrane with the average pore size of 300-500 nm is used as a base membrane, ceramic particles with the average particle size of 100-500 nm are used as coating filler, an inorganic binder is used as a sintering aid, a water-soluble high-molecular polymer is used as a dispersing agent, and a surfactant and a defoaming agent are used as auxiliary additives, and blade coating slurry is obtained after uniform mixing; and coating the slurry on the surface of a commercial ceramic membrane by adopting a blade coating method, and sintering to obtain a stable and non-falling ceramic membrane product in which ceramic particles and an inorganic adhesive are bonded by chemical bonds. The method is simple, convenient, few in steps, easy to operate and low in sintering temperature, and the prepared membrane has the advantages of being small in pore diameter (the pore diameter of 50-100 nm is adjustable), narrow in pore diameter distribution (the pore diameter of 50-100 nm accounts for not less than 95%), excellent in small-size oil drop separation performance, high in anti-pollution capacity and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic membrane separation, and particularly relates to a method and product for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance. Background Art

[0002] Oily wastewater is commonly produced in food processing, industrial production and other fields. Direct discharge of untreated wastewater will pose a serious threat to the ecosystem. The oil droplets in oily wastewater mainly exist in the form of free oil (>150μm), dispersed oil (25-150μm) and emulsified oil (<25μm). The free oil and dispersed oil droplets are easy to aggregate and be removed under the action of external forces; while the surface of emulsified oil droplets usually adsorbs surfactants and is relatively stable and not easy to aggregate, so it is more difficult to treat. Traditional methods for treating oily wastewater include adsorption, flocculation, biological treatment, gas flotation, etc. However, these methods have poor removal effects on stable small-sized emulsified oil droplets and are difficult to meet discharge requirements.

[0003] Compared with traditional oily wastewater treatment technologies, membrane separation technology has attracted much attention due to its advantages such as high separation accuracy, low cost and energy consumption. Although polymer membranes are low in cost, they are easily contaminated by oil adsorption, which reduces their service life and limits their application in oily wastewater. In addition, emulsified oil droplets will deform under pressure and easily pass through membranes with pore sizes smaller than the emulsified oil droplets. Compared with polymer membranes, inorganic membranes (especially ceramic membranes) have the advantages of high mechanical strength, good stability, low requirements for the use environment, and easy cleaning. However, commercially available ceramic membranes generally have large pore sizes (>200nm), wide pore size distribution, and complex preparation processes, which limit their application. In addition, ceramic membranes have poor separation performance and anti-oil pollution performance for small-sized emulsified oil wastewater.

[0004] At present, the surface pore size of the ceramic-based membrane can be effectively reduced by adopting the "surface layer coating-sintering" method. For example, Chinese invention CN111420562A discloses a method for preparing a hollow flat ceramic membrane. The invention adopts a multiple spraying method to evenly spray three layers of slurry on the surface of the ceramic support body, and obtains a ceramic membrane with an average pore size of 40nm and a porosity of 40% by high-temperature sintering. However, its application is limited by factors such as the complex preparation process and the need for multi-step processing, and the pore size distribution range of the membrane has not yet been clarified. Patent CN102701778B discloses a method for preparing a ceramic membrane with a multi-level pore structure. First, a variety of coating liquids are prepared with ceramic powder and pore-forming agent, and a ceramic membrane with a gradient distribution multi-level pore structure is obtained by multiple dipping-coating processes. Although the preparation method of the invention can achieve the pore size of the third separation layer in the range of 50 to 100nm, there are limitations such as long preparation time and high cost of the separation layer, and it cannot guarantee the firm bonding between multiple separation layers. Patent CN110368818B discloses a method for preparing a high-flux flat ceramic membrane. The invention uses a spray coating method to prepare an intermediate transition layer on the surface of the flat ceramic membrane support, and then uses a dip coating method to prepare a separation membrane layer. After sintering, an average pore size of 46nm and a water permeation flux of 420L m - 2 bar -1 h -1 Flat ceramic membrane. However, since the invention requires the combination of spraying technology and impregnation process, its preparation process has high technical requirements and many steps, which is not suitable for practical application. In addition, for the anti-oil pollution ability of ceramic membrane, "surface modification technology" can be used to improve the hydrophilicity and hydrophobicity of the membrane, so as to enhance the anti-pollution ability of ceramic membrane. For example, Chinese invention CN112121647A discloses that ceramic powder is pressed into a ceramic embryo by dry pressing, then immersed in a mixed solution of TEOS and PDMS, and then acid-treated after removal to obtain an oil-water separation ceramic membrane with super hydrophilic and super oleophobic properties. CN116283238A patent discloses a preparation technology of an oil-water separation ceramic membrane with stable performance and strong anti-pollution ability. The invention uses aluminum oxide and kaolin as the main raw materials, and forms an oleophobic layer constructed by mullite whiskers on the surface of the ceramic membrane through the catalytic action of ammonium molybdate, forming a super hydrophilic / underwater super oleophobic, oil-water separation effect The ceramic membrane has a good effect. Although the above methods improve the anti-fouling performance of ceramic membranes, their application is limited by factors such as complex preparation process, high technical requirements, repeated treatment, and easy attenuation of hydrophilicity. In addition, the uniformity of membrane pore size distribution and anti-fouling performance are still unclear. In summary, multiple coating processes can reduce the pore size of the membrane, but fail to simplify the shrinkage process, and it is still difficult to solve the bottleneck of wide pore size distribution. Although surface modification technology can improve the anti-fouling performance of the membrane, it is difficult to reduce the pore size of the membrane. Therefore, how to achieve simple and effective shrinkage of the pore size on the surface of the ceramic membrane, improve pore size uniformity and anti-fouling performance is the key to solving the poor efficiency of ceramic membranes in oil-water separation.

[0005] On the basis of the above limitations, the present invention adopts a scraping method to prepare a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance. Specifically, a commercial ceramic membrane with an average pore size of 300-500nm is used as a base membrane, ceramic particles with an average particle size of 100-500nm are used as coating fillers, an inorganic binder is used as a sintering aid, a water-soluble polymer is used as a dispersant, and a surfactant and a defoaming agent are used as auxiliary additives. After mixing, a scraping slurry is obtained, and the slurry is scraped on the surface of the commercial ceramic membrane by a scraping method. After sintering treatment, a stable and non-shedding ceramic membrane product is obtained in which the ceramic particles and the inorganic binder are chemically bonded. This method is not only simple, has few steps, is easy to operate, and has a low sintering temperature, but also the prepared membrane has the advantages of small pore size (adjustable pore size of 50-100nm), narrow pore size distribution (pore size of 50-100nm accounts for not less than 95%), excellent separation performance for small-sized oil droplets, and strong anti-pollution ability. Summary of the invention

[0006] In view of the existing problems, the present invention aims to provide a simple preparation method and product of a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance.

[0007] The technical solution of the present invention is a simple preparation method for a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance, which uses a commercial ceramic membrane with an average pore size of 300-500nm as a base membrane, ceramic particles with an average particle size of 100-500nm as a coating filler, an inorganic binder as a sintering aid, a water-soluble high molecular polymer as a dispersant, a surfactant and a defoaming agent as auxiliary additives, and the scraping slurry is obtained after mixing. The scraping method is used to prepare a small-pore ceramic membrane with "adjustable pore size in the range of 50-100nm and narrow pore size distribution (pore size of 50-100nm accounts for not less than 95%)".

[0008] The above-mentioned simple method for preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution performance has the following specific steps:

[0009] S1. Take ceramic particles, inorganic binder, dispersant, surfactant, defoamer and deionized water in a mass ratio of 20-50:4-30:10-16:0.1-1:0.1-2:25.8-31, add them into a mixer and mix and stir for 1-5 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0010] S2, after vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film under preset conditions, and dried at 40-100° C. for 12-24 hours until the coating is completely dry;

[0011] S3. Place the membrane in a muffle furnace and sinter it at a setting temperature of 800-1500° C. and keep it warm for 1-5 hours. After cooling in the furnace, take it out to obtain the desired ceramic membrane product.

[0012] In the aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance, the ceramic particles in step S1 are one of aluminum oxide, silicon dioxide, zirconium oxide, silicon carbide and kaolin.

[0013] In the aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance, the inorganic binder in step S1 is one of aluminum phosphate, magnesium phosphate, aluminum dihydrogen phosphate, silica sol and alumina colloid.

[0014] In the aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance, the dispersant in step S1 is one of polyvinyl alcohol, polyethylene glycol, carboxymethyl cellulose and polyvinyl pyrrolidone.

[0015] The aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance, in step S1, the dissolution temperature of the water-soluble high molecular polymer in the ceramic scraping slurry is 35-95° C., and the dissolution time is 1-2 hours.

[0016] The aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties, wherein the surfactant in step S1 is one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, sodium hexadecyl sulfate and sodium octadecyl sulfate.

[0017] In the aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution property, the defoaming agent in step S1 is one of polyethylene glycol fatty alcohol ether, glycerol polyoxypropylene ether, polypropylene glycol, polydimethylsiloxane and tributyl phosphate.

[0018] In the aforementioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties, the viscosity of the ceramic slurry in step S1 is controlled in the range of 300 to 450 mPa s.

[0019] The above-mentioned method for simply preparing a small pore size, narrow pore size distribution, and high anti-pollution ceramic membrane, the ceramic coating in step S2 is scraped at a preset condition of 30 mm to 2 m min -1 , the ambient temperature is 25-35℃, the ambient humidity is 20%-40%, and the scraping film thickness is 100-500μm.

[0020] The above-mentioned method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties, wherein the sintering procedure is set in step S3, and the sintering temperature of the ceramic membrane is 800-1500°C, so that the inorganic binder and the ceramic particles are chemically bonded to each other so that the coating and the base membrane are firmly connected; wherein the low-temperature heating stage is room temperature to 600°C, and the heating rate is 1-2°C min -1 ; The high temperature sintering stage is from 600℃ to the sintering end temperature (800~1500℃) with a 1~5℃min -1 The heating rate is set and the highest temperature is kept for 1 to 5 hours. After cooling in the furnace, a ceramic membrane with small pore size and narrow pore size distribution is obtained.

[0021] The product is obtained by the above-mentioned preparation method of the small pore size, narrow pore size distribution and high pollution resistance ceramic membrane.

[0022] Beneficial Effects of the Invention

[0023] The principle of a simple preparation of a small pore size, narrow pore size distribution, and high anti-pollution ceramic membrane described in the present invention is: in the preparation process of a small pore size, narrow pore size distribution, and high anti-pollution ceramic membrane, the inorganic binder is dehydrated at high temperature to generate MO oxide rich in covalent bonds, and MO can be bonded to the ceramic particles in the separation layer or the O and Al of the commercially available ceramic base membrane to form covalent bonds, and finally a small pore size, narrow pore size distribution ceramic membrane is obtained in which the separation layer and the ceramic base membrane are bonded by covalent bonds and the macropores on the base membrane surface are effectively filled. At the same time, the inorganic binder introduced on the membrane surface can make the ceramic particles bond at a lower temperature, so that the sintering temperature of the membrane is moderately reduced. In addition, the inorganic binder introduced on the membrane surface has strong hydrophilicity and negative charge, so that the membrane has stronger hydrophilicity and more negative charge. In the oil-water separation process, the surface of the emulsified oil droplets stabilized by the surfactant carries a certain amount of negative charge. When the emulsified oil droplets contact the membrane surface, the negative charge on the membrane surface will produce an electrostatic repulsion effect on the emulsified oil droplets. Secondly, the pore blocking effect of the inorganic binder can reduce the roughness of the membrane surface and affect the spreading behavior of the emulsified oil droplets on the membrane surface, thereby improving the anti-oil pollution ability of the ceramic membrane. Therefore, the synergistic effect of membrane size screening and electrostatic repulsion is used to achieve deep treatment of small-sized emulsified oil wastewater.

[0024] The advantages and positive effects of the present invention are: (1) The operation method is simple. Only a simple scraping method is needed to prepare a small-pore ceramic membrane with narrow pore size distribution and high anti-pollution (adjustable pore size of 50-100nm, pore size ratio of not less than 95%). The method is simple, has few steps, is easy to operate and has obvious effects, and the sintering temperature of the membrane is moderately reduced; (2) The membrane can achieve efficient purification of small-sized emulsified oil wastewater; (3) The membrane's ability to resist oil pollution is significantly improved; (4) It effectively solves many limitations in the ceramic preparation process, such as the separation layer is easy to fall off, the preparation process is complicated, and the sintering temperature is high. (5) The method is also applicable to ceramic membranes of various configurations such as flat plates, tubular, and multi-channel. DETAILED DESCRIPTION

[0025] The technical route of the present invention in the specific implementation process will be described in detail and completely. It should be noted that the implementation process and technical route of the present invention mentioned above are only a small part of the key achievements involved in the present invention, and all technical requirements are not listed in detail. Based on the specific implementation plan, all other specific embodiments obtained by other technicians under the technical route of the present invention without creative work are within the protection scope of the present invention.

[0026] Embodiment 1:

[0027] S1. Calculated by mass fraction, take 60 parts of ceramic particles (alumina) with an average particle size of 500 nm, 4 parts of inorganic binder (magnesium phosphate), 10 parts of dispersant (polyvinyl alcohol), 0.1 parts of surfactant (sodium lauryl sulfate), 0.1 parts of defoamer (polyethylene glycol fatty alcohol ether) and 25.8 parts of deionized water, add them into a mixer and mix and stir for 5 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0028] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 25°C at a scraping rate of 30 mm / min. -1 , the environmental humidity is 20%, the scraping film thickness is 100μm, and it is dried at 40℃ for 24h until the coating is completely dry;

[0029] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600°C, and the heating rate is 1°C min -1 ; Then, the high temperature sintering stage was carried out at 1℃ min -1 The temperature is heated from 600°C to 800°C at a heating rate and kept at 800°C for 5 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0030] According to the test, the 99nm pore size of the ceramic membrane accounts for 96.2%, the oil-water separation efficiency is 96.4%, and the flux recovery rate after ten cycles is 95.5%. The 497nm pore size of the flat ceramic base membrane used accounts for 27.9%, the oil removal efficiency is 28.4%, and the flux recovery rate after ten cycles is 30.2%.

[0031] Embodiment 2:

[0032] S1. Calculated by mass fraction, take 55 parts of ceramic particles (zirconium oxide) with an average particle size of 500 nm, 7 parts of inorganic binder (silica sol), 11 parts of dispersant (polyethylene glycol), 0.2 parts of surfactant (sodium dodecylbenzene sulfonate), 0.4 parts of defoaming agent (glycerol polyoxypropylene ether) and 26.4 parts of deionized water, add them into a mixer and mix and stir for 4 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0033] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 28°C at a scraping rate of 100 mm / min. 1 , the environmental humidity is 30%, the scraping film thickness is 200μm, and it is dried at 50℃ for 22h until the coating is completely dry;

[0034] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600°C, and the heating rate is 1°C min -1 ; Then, the high temperature sintering stage, 1℃min -1 The temperature is heated from 600°C to 900°C at a heating rate and kept at 900°C for 5 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0035] According to the test, the pore size of the ceramic membrane is 97nm, accounting for 95.7%, the oil-water separation efficiency is 96.8%, and the flux recovery rate after ten cycles is 95.9%. The pore size of the flat ceramic base membrane used is 497nm, accounting for 27.9%, the oil removal efficiency is 28.4%, and the flux recovery rate after ten cycles is 30.2%.

[0036] Embodiment 3:

[0037] S1. Calculated by mass fraction, take 50 parts of ceramic particles (silicon carbide particles) with an average particle size of 400 nm, 10 parts of inorganic binder (alumina colloid), 12 parts of dispersant (carboxymethyl cellulose), 0.3 parts of surfactant (hexadecyltrimethylammonium bromide), 0.7 parts of defoaming agent (polypropylene glycol) and 27 parts of deionized water, add them into a mixer and mix and stir for 4 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0038] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 30°C at a scraping rate of 300 mm / min.-1 , the environmental humidity is 30%, the scraping film thickness is 200μm, and it is dried at 60℃ for 20h until the coating is completely dry;

[0039] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600°C, and the heating rate is 1°C min -1 ; Then, the high temperature sintering stage, 2℃min -1 The temperature is heated from 600°C to 1000°C at a heating rate and kept at 1000°C for 4 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0040] According to the test, the pore size of the ceramic membrane is 89nm, accounting for 97.4%, the oil-water separation efficiency is 98.1%, and the flux recovery rate after ten cycles is 97.3%. The pore size of the multi-channel flat ceramic base membrane used is 425nm, accounting for 37.8%, the oil removal efficiency is 35.4%, and the flux recovery rate after ten cycles is 36.1%.

[0041] Embodiment 4:

[0042] S1. Calculated by mass fraction, take 45 parts of ceramic particles (kaolin) with an average particle size of 400 nm, 13 parts of inorganic binder (aluminum phosphate), 13 parts of dispersant (polyvinyl alcohol), 0.4 parts of surfactant (sodium hexadecyl sulfate), 1 part of defoamer (polydimethylsiloxane) and 27.6 parts of deionized water, mix and stir in a mixer for 3 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0043] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 32°C at a scraping rate of 500 mm / min. -1 , the environmental humidity is 40%, the scraping film thickness is 300μm, and it is dried at 70℃ for 18h until the coating is completely dry;

[0044] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600 °C, and the heating rate is 2 °C min -1 ; Then, the high temperature sintering stage, 2℃min -1 The temperature is heated from 600°C to 1100°C at a heating rate and kept at 1100°C for 3 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0045] According to the test, the pore size of the ceramic membrane is 86nm, accounting for 96.9%, the oil-water separation efficiency is 98.5%, and the flux recovery rate after ten cycles is 97.4%. The pore size of the multi-channel flat ceramic base membrane used is 425nm, accounting for 37.8%, the oil removal efficiency is 35.4%, and the flux recovery rate after ten cycles is 36.1%.

[0046] Embodiment 5:

[0047] S1. Calculated by mass fraction, take 40 parts of ceramic particles (silicon dioxide) with an average particle size of 300 nm, 16 parts of inorganic binder (aluminum dihydrogen phosphate), 14 parts of dispersant (polyvinyl pyrrolidone), 0.5 parts of surfactant (sodium octadecyl sulfate), 1.3 parts of defoaming agent (tributyl phosphate) and 28.2 parts of deionized water, mix and stir in a mixer for 2 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0048] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 35°C at a scraping rate of 800 mm / min. -1 , the environmental humidity is 30%, the scraping film thickness is 200μm, and it is dried at 80℃ for 16h until the coating is completely dry;

[0049] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is room temperature to 600°C, and the heating rate is 2°C min -1 ; Then, the high temperature sintering stage was carried out at 3℃ min -1 The temperature is heated from 600°C to 1200°C at a heating rate and kept at 1200°C for 2 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0050] According to the test, the pore size of the ceramic membrane is 70nm, accounting for 97.9%, the oil-water separation efficiency is 98.6%, and the flux recovery rate after ten cycles is 97.8%. The pore size of the flat ceramic base membrane used is 363nm, accounting for 44.1%, the oil removal efficiency is 43.7%, and the flux recovery rate after ten cycles is 40.5%.

[0051] Embodiment 6:

[0052] S1. Calculated by mass fraction, take 35 parts of ceramic particles (silicon dioxide) with an average particle size of 300 nm, 20 parts of inorganic binder (alumina colloid), 14 parts of dispersant (polyvinyl alcohol), 0.6 parts of surfactant (sodium hexadecyl sulfate), 1.5 parts of defoaming agent (glycerol polyoxypropylene ether) and 28.9 parts of deionized water, mix and stir in a mixer for 2 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0053] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 25°C at a scraping rate of 1m min -1 , the environmental humidity is 20%, the scraping film thickness is 300μm, and it is dried at 90℃ for 15h until the coating is completely dry;

[0054] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600 °C, and the heating rate is 2 °C min -1 ; Then, the high temperature sintering stage was carried out at 3℃ min -1 The temperature is heated from 600°C to 1300°C at a heating rate and kept at 1300°C for 3 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0055] According to the test, the pore size of the ceramic membrane is 68nm, accounting for 97.2%, the oil-water separation efficiency is 99.2%, and the flux recovery rate after ten cycles is 98.5%. The pore size of the flat ceramic base membrane used is 363nm, accounting for 44.1%, the oil removal efficiency is 43.7%, and the flux recovery rate after ten cycles is 40.5%.

[0056] Embodiment 7:

[0057] S1. Calculated by mass fraction, take 30 parts of ceramic particles (kaolin) with an average particle size of 200 nm, 23 parts of inorganic binder (silica sol), 15 parts of dispersant (polyvinyl pyrrolidone), 0.7 parts of surfactant (sodium octadecyl sulfate), 1.7 parts of defoaming agent (polydimethylsiloxane) and 29.6 parts of deionized water, mix and stir in a mixer for 1 hour to obtain a uniform coating or coating slurry with moderate viscosity;

[0058] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 28°C at a scraping rate of 1m min -1 , the environmental humidity is 30%, the scraping film thickness is 300μm, and it is dried at 90℃ for 14h until the coating is completely dry;

[0059] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600 °C, and the heating rate is 2 °C min -1 Subsequently, the high temperature sintering stage was carried out at 4 °C min -1 The temperature is heated from 600°C to 1400°C at a heating rate and kept at 1400°C for 2 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0060] According to the test, the ceramic membrane with a pore size of 59nm accounts for 97%, the oil-water separation efficiency is 100%, and the flux recovery rate after ten cycles is 98.6%. The flat ceramic base membrane with a pore size of 327nm accounts for 47.2%, the oil removal efficiency is 46.5%, and the flux recovery rate after ten cycles is 41.8%.

[0061] Embodiment 8:

[0062] S1. Calculated by mass fraction, take 25 parts of ceramic particles (zirconium oxide) with an average particle size of 200 nm, 26 parts of inorganic binder (aluminum dihydrogen phosphate), 15 parts of dispersant (polyvinyl alcohol), 0.8 parts of surfactant (sodium dodecylbenzene sulfonate), 1.9 parts of defoamer (polyethylene glycol fatty alcohol ether) and 31.3 parts of deionized water, mix and stir in a mixer for 3 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0063] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 30°C at a scraping rate of 2 m / min. -1 , the environmental humidity is 30%, the scraping film thickness is 500μm, and it is dried at 95℃ for 13h until the coating is completely dry;

[0064] S3. The membrane is then placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is from room temperature to 600°C, and the heating rate is 1°C min -1 ; Then, the high temperature sintering stage was carried out at 4℃min -1 The temperature is heated from 600°C to 1450°C at a heating rate and kept at 1450°C for 2 hours. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0065] According to the test, the ceramic membrane with a pore size of 57nm accounts for 97.9%, the oil-water separation efficiency is 100%, and the flux recovery rate after ten cycles is 98.1%. The flat ceramic base membrane with a pore size of 327nm accounts for 47.2%, the oil removal efficiency is 46.5%, and the flux recovery rate after ten cycles is 41.8%.

[0066] Embodiment 9:

[0067] S1. Calculated by mass fraction, take 20 parts of ceramic particles (zirconium oxide) with an average particle size of 100 nm, 30 parts of inorganic binder (silica sol), 16 parts of dispersant (polyethylene glycol), 1 part of surfactant (sodium hexadecyl sulfate), 2 parts of defoaming agent (tributyl phosphate) and 31 parts of deionized water, mix and stir in a mixer for 3 hours to obtain a uniform coating or coating slurry with moderate viscosity;

[0068] S2. After vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film at 35°C at a scraping rate of 1m min -1 , the environmental humidity is 30%, the scraping film thickness is 400 μm, and it is dried at 100°C for 12 hours until the coating is completely dry;

[0069] S3, then the membrane is placed in a muffle furnace and sintered under a set program; first, the low-temperature sintering stage is room temperature ~ 600 ° C, and the heating rate is 1 ° C min -1 ; Then, the high temperature sintering stage, 5℃min -1The temperature is heated from 600°C to 1500°C at a heating rate and kept at 1500°C for 1 hour. After cooling in the furnace, the desired ceramic membrane product is obtained.

[0070] According to the test, the ceramic membrane with a pore size of 50nm accounts for 98.3%, the oil-water separation efficiency is 100%, and the flux recovery rate after ten cycles is 98.9%. The flat ceramic base membrane with a pore size of 305nm accounts for 47.2%, the oil removal efficiency is 49.2%, and the flux recovery rate after ten cycles is 51.8%.

Claims

1. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties, characterized in that: A commercial ceramic membrane with an average pore size of 300-500nm is used as the base membrane, ceramic particles with an average particle size of 100-500nm are used as the coating filler, an inorganic binder is used as a sintering aid, a water-soluble high molecular polymer is used as a dispersant, and a surfactant and a defoaming agent are used as auxiliary additives. After mixing, a scraping slurry is obtained, and a scraping method is used to prepare a small-pore ceramic membrane with "adjustable pore size in the range of 50-100nm and narrow pore size distribution (pore size of 50-100nm accounts for not less than 95%)".

2. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties, characterized in that: The specific steps are as follows: S1. Take ceramic particles, inorganic binder, water-soluble high polymer, surfactant, defoamer and deionized water in a mass ratio of 20-60:4-30:10-16:0.1-1:0.1-2:25.8-31, add them into a mixer and mix and stir for 1-5 hours to obtain a uniform coating or coating slurry with moderate viscosity; S2, after vacuum degassing, the obtained slurry is scraped on the surface of the ceramic base film under preset conditions, and dried at 40-100° C. for 12-24 hours until the coating is completely dry; S3. Place the membrane in a muffle furnace and sinter it at a setting temperature of 800-1500° C. and keep it warm for 1-5 hours. After cooling in the furnace, take it out to obtain the desired ceramic membrane product.

3. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The ceramic particles in step S1 are one of alumina, silica, zirconium oxide, silicon carbide and kaolin.

4. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The inorganic binder in step S1 is one of aluminum phosphate, magnesium phosphate, aluminum dihydrogen phosphate, silica sol, and alumina colloid.

5. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The dispersant in step S1 is one of polyvinyl alcohol, polyethylene glycol, carboxymethyl cellulose and polyvinyl pyrrolidone.

6. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The dissolution temperature of the water-soluble high molecular polymer in the ceramic scraping slurry in step S1 is 35-95° C., and the dissolution time is 1-2 hours.

7. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The surfactant in step S1 is one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, sodium hexadecyl sulfate, and sodium octadecyl sulfate.

8. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The defoaming agent in step S1 is one of polyethylene glycol fatty alcohol ether, glycerol polyoxypropylene ether, polypropylene glycol, polydimethylsiloxane, and tributyl phosphate.

9. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The viscosity of the ceramic slurry in step S1 is controlled in the range of 300 to 450 mPa s.

10. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: The preset conditions for scraping the ceramic coating in step S2 are that the scraping rate is 30 mm to 2 m min -1 , the ambient temperature is 25-35℃, the ambient humidity is 20%-40%, and the scraping film thickness is 100-500μm.

11. A method for simply preparing a ceramic membrane with small pore size, narrow pore size distribution and high anti-pollution properties according to claim 2, characterized in that: In the sintering procedure of step S3, the sintering temperature of the ceramic film is 800-1500°C, so that the inorganic binder and the ceramic particles are chemically bonded to firmly connect the coating and the base film; wherein, the low temperature heating stage is room temperature to 600°C, and the heating rate is 1-2°C min -1 ; The high temperature sintering stage is from 600℃ to the sintering end temperature (800~1500℃) with a 1~5℃min -1 The heating rate is set and the highest temperature is kept for 1 to 5 hours. After cooling in the furnace, a ceramic membrane with small pore size and narrow pore size distribution is obtained.

12. A product obtained by the method for preparing a ceramic membrane with small pore size, narrow pore size distribution and high pollution resistance as described in claim 1 or 2.

Citation Information

Patent Citations

  • Flat ceramic membrane and preparation method thereof

    CN111545078A

  • Ceramic membrane as well as preparation method and application thereof

    CN115999381A

  • Method for preparing gas-solid separation ceramic membrane based on phase inversion method and spraying method

    CN117504619A

  • Method for manufacturing porous clay-based ceramic membrane with ceramic coating layer and ceramic membrane manufactured thereby

    KR1020150092518A

  • Porous inorganic membrane with reactive inorganic binder, and method of forming same

    WO1989011342A1

Cited By

  • Underwater super-oleophobic alumina ceramic microfiltration membrane and preparation method and application thereof

    CN119588178A

  • Rare earth doped antibacterial nano ceramic membrane as well as preparation method and application thereof