A water-soluble binder for lithium-ion batteries and its preparation method and application

By using water-soluble binders prepared by materials such as modified carbon nanotubes and tanninic acid in lithium-ion batteries, the structural damage caused by volume changes of silicon negative electrode materials is solved, and the cycle stability and electrochemical performance of the battery are improved. , extends battery life.

CN115172753BActive Publication Date: 2024-11-26WUXI LINGYI FUTURE RES INST OF NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210966680.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-12
Publication Date
2024-11-26
Estimated Expiration
2042-08-12

AI Technical Summary

Technical Problem

The structure damage and irreversible capacity loss caused by volume changes during the charging and discharge process of the silicon negative electrode material of lithium-ion batteries affect the cycle stability and life of the battery. Existing adhesives such as PVDF are difficult to withstand huge volume expansion, resulting in the disintegration of the electrode layer. and capacity decline.

Method used

Using a preparation method of a lithium-ion battery water-soluble binder, carbon nanotubes, tanninic acid and other monomers are polymerized under the action of an initiator to form a crosslinked copolymer, and the pH is adjusted with lithium hydroxide. A binder with strong interfacial interaction and good dispersion is obtained to enhance the bonding strength and stability of the electrode material.

Benefits of technology

It significantly improves the cycle life and electrochemical performance of lithium-ion batteries, enhances the peel strength and heat resistance of electrode materials, alleviates the structural instability caused by volume expansion of silicon particles, and extends the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172753B_ABST
    Figure CN115172753B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, and discloses a water-soluble binder for lithium ion batteries, a preparation method thereof and an application thereof. Carbon nanotubes are olefin-modified, and then, after polymerization reaction is carried out with acrylonitrile monomers, N,N-diethyl-2-acrylamide monomers, acrylic acid monomers and tannic acid monomers under the action of an initiator, the monomers react with isocyanate groups of isocyanate-terminated polyurethane to obtain a water-soluble binder for lithium ion batteries. The water-soluble binder has the advantages of being green and environmentally friendly. The obtained water-soluble binder improves the dispersibility of carbon nanotubes, is conducive to the transmission of electrons, and gives the binder excellent toughness and mechanical strength. The water-soluble binder has a three-dimensional network structure, good adhesion, good heat resistance, can adapt to the volume expansion and contraction of silicon-based negative electrode materials, can still maintain structural stability after a huge volume change occurs, thereby enhancing the cycle performance of the battery, thereby effectively extending the battery life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a water-soluble binder for lithium ion batteries and a preparation method and application thereof. Background Art

[0002] With the gradual depletion of fossil energy and the rapid development of modern science and technology, energy issues have become a major theme in the development of the world today. Lithium-ion batteries, as a green energy with broad development prospects, have the characteristics of high safety performance, good cycle stability and easy use. They are widely used in portable electronic products, electric vehicles, drones, energy storage batteries and other fields.

[0003] The problems of "battery life and charging" in lithium-ion battery application products have placed higher and higher requirements on the energy density of lithium-ion batteries. Among them, the negative electrode material of lithium-ion batteries plays a key role in lithium-ion batteries. During the charging and discharging process, the negative electrode material of lithium-ion batteries constantly reacts with lithium ions. As the most mature carbon-based negative electrode active material, graphite has basically fully utilized its specific capacity. Among the potential negative electrode materials for lithium-ion batteries, silicon materials have attracted much attention because of their theoretical specific capacity of up to 4200mAh / g, abundant reserves and controllable costs. Using silicon materials as negative electrode materials can effectively increase the energy density of batteries and reduce the manufacturing cost of batteries. However, silicon materials do not have a layered crystal structure. They store lithium ions by forming lithium-silicon alloys. In the process of lithium ion insertion and extraction, the Li 15 Si 4 The transformation between amorphous silicon and silicon involves severe volume expansion and contraction, resulting in large volume changes.

[0004] At present, the various components of silicon negative electrode materials are bonded together by a binder, and their mechanical strength is limited. The stress generated by the volume change of silicon materials during the cycle will destroy the structure of the silicon negative electrode, causing the contact between the active material and the conductive agent to be separated and the conductive network to collapse, thereby affecting the cycle stability of the battery. In addition, the volume expansion of the silicon negative electrode will also destroy the solid electrolyte layer between the electrolyte and the pole piece. In this process, a large amount of lithium ions and electrolyte will be consumed, resulting in irreversible capacity loss, thereby affecting the life of the lithium-ion battery.

[0005] The effective bonding of the binder to the electrode material is divided into two steps: "penetration" and "hardening". During the penetration process, the binder will infiltrate the surface of the electrode material and penetrate into it through the microporous structure of the electrode material surface, thereby fully contacting the electrode material; during the hardening process, the binder hardens through physical and chemical reactions, and the electrode particles and the binder are combined through mechanical interlocking and interfacial interaction forces to form a joint, completing the bonding. The mechanical strength of the binder is affected by the mechanical interlocking effect, interfacial interaction force, the mechanical strength of the binder, and the mechanical strength of the electrode material. Therefore, strengthening the mechanical interlocking effect and interfacial interaction force can improve the bonding strength. Currently known methods for strengthening interfacial interaction forces are: (1) strengthening hydrogen bond interaction forces; (2) introducing electrostatic interaction forces through ionic bonds; (3) forming covalent bonds between the binder and the active material.

[0006] Chinese patent application CN112310399A discloses a lithium-ion battery silicon negative electrode binder and its electrode preparation method and application. The lithium-ion battery silicon negative electrode binder is composed of polyvinylidene fluoride (PVDF) and polyvinyl alcohol. On the basis of improving the overall adhesion of the electrode, it effectively suppresses the irreversible lithium consumption of the electrode, but its effect of improving the adhesion of the electrode is general. At present, the scientific community has determined that the large volume change of silicon during repeated charge and discharge cycles is the main source of the insufficient cycle life of the silicon negative electrode. The weak van der Waals interaction between the traditional polyvinylidene fluoride binder and silicon is difficult to withstand the huge volume expansion of silicon during the charge and discharge process. The electrode layer structure will disintegrate, and it will also cause the electrode layer to fall off from the conductive current collector, resulting in the cyclic decay of the electrode capacity. Therefore, the PVDF binder, which currently occupies the mainstream position in industrialization, is not suitable for silicon negative electrodes and the current development application needs. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a water-soluble binder for lithium-ion batteries and a preparation method and application thereof, so as to improve the stripping force and electrochemical performance of the original material.

[0008] In order to achieve the above object, the present invention discloses a method for preparing a water-soluble binder for lithium-ion batteries, comprising the following steps:

[0009] Step 1, anhydrous ethanol, carbon nanotubes, and γ-methacryloxypropyltrimethoxysilane are stirred and mixed, heated to react, and after the reaction is completed, cooled and filtered, the filter residue is washed with ethanol, and vacuum dried at 60-65° C. for 6-10 hours to obtain olefin-modified carbon nanotubes;

[0010] Step 2, deionized water and tannic acid are mixed evenly, and then olefin-modified carbon nanotubes, acrylonitrile, N,N-diethyl-2-acrylamide, and acrylic acid are added, stirred and mixed, potassium hydroxide is added to adjust the pH to 4-5, an initiator is added, and heating is performed to react. After the reaction is completed, drying is performed at a drying temperature of 75-85° C. and a reaction time of 10-15 hours to obtain a multi-polymer;

[0011] Step 3: Evenly mix N,N-dimethylformamide, multi-polymer and stannous octoate, add isocyanate-terminated polyurethane in a nitrogen atmosphere, and react during heating and reflux. After the reaction is completed, cool, precipitate with petroleum ether, filter, and vacuum dry at 50-60°C for 8-12h to obtain a cross-linked copolymer, add deionized water to the cross-linked copolymer, adjust the pH to 7-8 with lithium hydroxide, stir and mix, and obtain a water-soluble binder for lithium-ion batteries.

[0012] Preferably, in the step 1, the mass ratio of anhydrous ethanol, carbon nanotubes and γ-methacryloxypropyltrimethoxysilane is 3500-5500:100:85-150.

[0013] Preferably, the reaction temperature in step 1 is 60-70° C., and the reaction time is 18-24 h.

[0014] Preferably, in step 2, the mass ratio of deionized water, tannic acid, olefin-modified carbon nanotubes, acrylonitrile, N,N-diethyl-2-acrylamide, acrylic acid, and initiator is 1800-3500:100:3-10:8-30:15-50:12-35:3-8.

[0015] Preferably, the reaction temperature in step 2 is 50-65° C., and the reaction time is 3-8 h.

[0016] Preferably, the initiator in step 2 comprises one of potassium persulfate, benzoyl peroxide and ammonium persulfate.

[0017] Preferably, in step 3, the mass ratio of N,N-dimethylformamide, multi-polymer, stannous octoate and isocyanate-terminated polyurethane is 400-900:100:0.5-1:35-75.

[0018] Preferably, the reaction temperature in step 3 is 75-90° C., and the reaction time is 5-12 h.

[0019] Preferably, in step three, the mass ratio of deionized water to the cross-linked copolymer is 100:10-25.

[0020] Preferably, in step 3, the stirring temperature is 60-80° C., the stirring time is 2-5 h, and the stirring rate is 1200-1800 rpm.

[0021] Preferably, the water-soluble binder for lithium-ion batteries prepared by the method for preparing a water-soluble binder for lithium-ion batteries.

[0022] A lithium ion battery, the preparation of which includes the lithium ion battery water-soluble binder prepared by the above method.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. In the present invention, γ-methacryloxypropyltrimethoxysilane is used to modify carbon nanotubes to obtain alkenyl-modified carbon nanotubes. The alkenyl-modified carbon nanotubes, acrylonitrile monomers, N,N-diethyl-2-acrylamide monomers, acrylic acid monomers and tannic acid monomers undergo polymerization reaction under the action of an initiator to obtain a multi-polymer. In a nitrogen atmosphere, the hydroxyl groups in the multi-polymer react with the isocyanate groups of the isocyanate-terminated polyurethane to obtain a cross-linked copolymer. After the cross-linked copolymer and deionized water are stirred and mixed, a water-soluble binder for lithium-ion batteries is obtained under the action of lithium hydroxide, which has the advantage of being green and environmentally friendly.

[0025] 2. In the present invention, the carbon nanotubes are polymerized with other monomers by polymerization, which effectively improves the dispersibility of the carbon nanotubes, avoids the agglomeration of the carbon nanotubes in the binder, and can be evenly dispersed. The carbon nanotubes have excellent electronic conductivity and can form a continuous conductive network in the electrode active material, which can greatly improve the penetration of the electrolyte in the electrode material and is beneficial to the transmission of electrons. At the same time, the carbon nanotubes have excellent toughness and mechanical strength, which can improve the peeling caused by the volume change of the material during the charge and discharge process, and can greatly improve the cycle life of the lithium-ion battery.

[0026] 3. The acrylic acid monomer used in the present invention contains a large number of carboxyl functional groups, which can generate hydrogen bonds with strong interactions with silicon electrodes, establish strong interfacial interactions, and enhance the adhesion of nano-silicon particles to the current collector, promote the formation of a thin and dense solid electrolyte interface film on the electrode surface, reduce the decomposition of the electrolyte on the electrode surface, and thus significantly improve the electrochemical performance.

[0027] 4. The tannic acid used in the present invention has abundant polar structures such as phenolic hydroxyl and carbonyl, has strong hydrophilicity and reactivity, and the multi-polymer prepared by polymerization reaction has strong electrostatic adsorption. The prepared aqueous binder has good water solubility and can be applied to the preparation process of lithium ion battery electrode sheets to improve the uniformity of electrode slurry, so that the electrode slurry can be formed into a film uniformly and flatly on the current collector; it can enhance the bonding strength between the electrode active material, the conductive agent and the current collector, which is beneficial to the conduction of electrons / ions during the charge and discharge process, reduces the electrochemical interface impedance of the electrode sheet, and significantly improves the electrochemical performance of the binder. The silicon electrode assembled using the water-soluble binder has improved long-term cycle performance at higher current density and charge and discharge performance at high rate current, which is beneficial to the transmission of ions, improves the bonding force when polyacrylic acid is used alone, the overall stability of the electrode material and the wettability of the binder to the electrode material, and greatly improves the peeling strength of the electrode.

[0028] 5. In the present invention, isocyanate-terminated polyurethane is added to react with the hydroxyl group on tannic acid to obtain a cross-linked copolymer having a three-dimensional network structure. Through entanglement and chemical action between molecules, a cross-linked copolymer containing hydrophilicity and functionality is obtained, which has good adhesion and supporting mechanical properties, and better heat resistance. This special structure has high adhesion, high mechanical strength and self-healing properties to silicon electrodes, can effectively adapt to the volume expansion and contraction of silicon-based negative electrode materials, and can still maintain structural stability after a huge volume change. As a negative electrode binder for lithium-ion batteries, it can improve the cycle stability of the battery, alleviate the powder shedding phenomenon caused by the volume expansion of silicon particles, and further enhance the cycle performance of the battery, thereby effectively extending the battery life. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a flow chart of preparing a water-soluble binder for lithium-ion batteries in the present invention;

[0030] Figure 2 This is a test diagram of the capacity retention rate of the lithium-ion battery in the present invention.

[0031] In the figure: 1, sample one; 2, sample two; 3, sample three; 4, comparison sample one; 5, comparison sample two; 6, comparison sample three. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] Embodiment 1

[0034] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0035] (1) 10 g of carbon nanotubes were added to 350 g of anhydrous ethanol, stirred and mixed evenly, and then 8.5 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 60° C. for 24 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and vacuum dried at 60° C. for 10 h to obtain olefin-modified carbon nanotubes;

[0036] (2) 10 g of tannic acid was added to 180 g of deionized water, and mixed evenly. Then, 0.3 g of olefin-modified carbon nanotubes, 0.8 g of acrylonitrile, 1.5 g of N,N-diethyl-2-acrylamide, and 1.2 g of acrylic acid were added, and stirred and mixed. Potassium hydroxide was added to adjust the pH to 4, and 0.3 g of initiator potassium persulfate was added. The mixture was heated to react at a temperature of 50° C. for 8 h. After the reaction was completed, the mixture was dried at a temperature of 75° C. for 15 h to obtain a multi-polymer.

[0037] (3) 40 g of N,N-dimethylformamide, 10 g of multi-polymer, and 0.05 g of stannous octoate were mixed evenly, and 3.5 g of isocyanate-terminated polyurethane was added in a nitrogen atmosphere. The reaction occurred during heating and reflux. The reaction temperature was 75° C. and the reaction time was 12 h. After the reaction was completed, the mixture was cooled, precipitated with petroleum ether, filtered, and vacuum dried at 50° C. for 12 h to obtain a cross-linked copolymer. 2 g of the cross-linked copolymer was added to 20 g of deionized water, the pH was adjusted to 7 with lithium hydroxide, and the mixture was stirred at a temperature of 60° C., a stirring time of 5 h, and a stirring rate of 1200 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0038] Embodiment 2

[0039] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0040] (1) 10 g of carbon nanotubes were added to 450 g of anhydrous ethanol, stirred and mixed evenly, and then 12 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 65° C. for 20 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and dried under vacuum at 60° C. for 8 h to obtain olefin-modified carbon nanotubes;

[0041] (2) 10 g of tannic acid was added to 280 g of deionized water, and mixed evenly. Then, 0.7 g of olefin-modified carbon nanotubes, 2 g of acrylonitrile, 3.5 g of N,N-diethyl-2-acrylamide, and 2.5 g of acrylic acid were added, and stirred and mixed. Potassium hydroxide was added to adjust the pH to 4.5, and 0.6 g of initiator potassium persulfate was added. The mixture was heated to react at a temperature of 65° C. for 5 h. After the reaction was completed, the mixture was dried at a temperature of 80° C. for 12 h to obtain a multi-polymer.

[0042] (3) 70 g of N,N-dimethylformamide, 10 g of multi-polymer, and 0.08 g of stannous octoate were mixed evenly, and 6 g of isocyanate-terminated polyurethane was added in a nitrogen atmosphere. The reaction occurred during heating and reflux. The reaction temperature was 85° C. and the reaction time was 10 h. After the reaction was completed, the mixture was cooled, precipitated with petroleum ether, filtered, and vacuum dried at 55° C. for 10 h to obtain a cross-linked copolymer. 3.5 g of the cross-linked copolymer was added to 20 g of deionized water, the pH was adjusted to 7.5 with lithium hydroxide, and the mixture was stirred at a temperature of 75° C., a stirring time of 4 h, and a stirring rate of 1500 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0043] Embodiment 3

[0044] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0045] (1) 10 g of carbon nanotubes were added to 550 g of anhydrous ethanol, stirred and mixed evenly, and then 15 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 70° C. for 18 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and vacuum dried at 65° C. for 6 h to obtain olefin-modified carbon nanotubes;

[0046] (2) 10 g of tannic acid was added to 350 g of deionized water and mixed evenly, and then 1 g of olefin-modified carbon nanotubes, 3 g of acrylonitrile, 5 g of N,N-diethyl-2-acrylamide, and 3.5 g of acrylic acid were added and stirred, potassium hydroxide was added to adjust the pH to 5, and 0.8 g of initiator potassium persulfate was added, and heated to react at a temperature of 65° C. for 3 h. After the reaction was completed, the mixture was dried at a temperature of 85° C. for 10 h to obtain a multi-polymer;

[0047] (3) 90 g of N,N-dimethylformamide, 10 g of multi-polymer, and 0.1 g of stannous octoate were mixed evenly, and 7.5 g of isocyanate-terminated polyurethane was added in a nitrogen atmosphere. The mixture was heated under reflux and reacted at a temperature of 90° C. for 5 h. After the reaction was completed, the mixture was cooled, precipitated with petroleum ether, filtered, and vacuum dried at 60° C. for 8 h to obtain a cross-linked copolymer. 5 g of the cross-linked copolymer was added to 20 g of deionized water, the pH was adjusted to 8 with lithium hydroxide, and the mixture was stirred at a temperature of 80° C. for 2 h and a stirring rate of 1800 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0048] Embodiment 4

[0049] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0050] (1) 10 g of carbon nanotubes were added to 450 g of anhydrous ethanol, stirred and mixed evenly, and then 12 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 65° C. for 20 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and dried under vacuum at 60° C. for 8 h to obtain olefin-modified carbon nanotubes;

[0051] (2) 10 g of tannic acid was added to 280 g of deionized water and mixed evenly, and then 0.7 g of olefin-modified carbon nanotubes, 2 g of acrylonitrile, 3.5 g of N,N-diethyl-2-acrylamide, and 2.5 g of acrylic acid were added and stirred, potassium hydroxide was added to adjust the pH to 4.5, and 0.6 g of initiator benzoyl peroxide was added, and heated to react at a temperature of 65° C. for 5 h. After the reaction was completed, the mixture was dried at a temperature of 80° C. for 12 h to obtain a multi-polymer;

[0052] (3) 70 g of N,N-dimethylformamide, 10 g of multi-polymer, and 0.08 g of stannous octoate were mixed evenly, and 6 g of isocyanate-terminated polyurethane was added in a nitrogen atmosphere. The reaction occurred during heating and reflux. The reaction temperature was 85° C. and the reaction time was 10 h. After the reaction was completed, the mixture was cooled, precipitated with petroleum ether, filtered, and vacuum dried at 55° C. for 10 h to obtain a cross-linked copolymer. 3.5 g of the cross-linked copolymer was added to 20 g of deionized water, the pH was adjusted to 7.5 with lithium hydroxide, and the mixture was stirred at a temperature of 75° C., a stirring time of 4 h, and a stirring rate of 1500 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0053] Embodiment 5

[0054] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0055] (1) 10 g of carbon nanotubes were added to 450 g of anhydrous ethanol, stirred and mixed evenly, and then 12 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 65° C. for 20 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and dried under vacuum at 60° C. for 8 h to obtain olefin-modified carbon nanotubes;

[0056] (2) 10 g of tannic acid was added to 280 g of deionized water and mixed evenly, and then 0.7 g of olefin-modified carbon nanotubes, 2 g of acrylonitrile, 3.5 g of N,N-diethyl-2-acrylamide, and 2.5 g of acrylic acid were added and stirred, potassium hydroxide was added to adjust the pH to 4.5, and 0.6 g of initiator ammonium persulfate was added, and heated to react at a temperature of 65° C. for 5 h. After the reaction was completed, the mixture was dried at a temperature of 80° C. for 12 h to obtain a multi-polymer;

[0057] (3) 70 g of N,N-dimethylformamide, 10 g of multi-polymer, and 0.08 g of stannous octoate were mixed evenly, and 6 g of isocyanate-terminated polyurethane was added in a nitrogen atmosphere. The reaction occurred during heating and reflux. The reaction temperature was 85° C. and the reaction time was 10 h. After the reaction was completed, the mixture was cooled, precipitated with petroleum ether, filtered, and vacuum dried at 55° C. for 10 h to obtain a cross-linked copolymer. 3.5 g of the cross-linked copolymer was added to 20 g of deionized water, the pH was adjusted to 7.5 with lithium hydroxide, and the mixture was stirred at a temperature of 75° C., a stirring time of 4 h, and a stirring rate of 1500 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0058] Comparative Example 1

[0059] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0060] (1) 10 g of carbon nanotubes were added to 550 g of anhydrous ethanol, stirred and mixed evenly, and then 15 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 70° C. for 18 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and vacuum dried at 65° C. for 6 h to obtain olefin-modified carbon nanotubes;

[0061] (2) 1 g of olefin-modified carbon nanotubes, 3 g of acrylonitrile, 5 g of N,N-diethyl-2-acrylamide, and 3.5 g of acrylic acid were added to 350 g of deionized water, stirred and mixed, potassium hydroxide was added to adjust the pH to 5, 0.8 g of initiator potassium persulfate was added, and heated to react at a temperature of 65° C. for 3 h. After the reaction was completed, the mixture was dried at a temperature of 85° C. for 10 h to obtain a multi-polymer;

[0062] (3) 5 g of the multi-polymer was added to 20 g of deionized water, the pH was adjusted to 8 using lithium hydroxide, and the mixture was stirred at a temperature of 80° C. for 2 h at a rate of 1800 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0063] Comparative Example 2

[0064] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0065] (1) 10 g of carbon nanotubes were added to 550 g of anhydrous ethanol, stirred and mixed evenly, and then 15 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 70° C. for 18 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and vacuum dried at 65° C. for 6 h to obtain olefin-modified carbon nanotubes;

[0066] (2) 3 g of acrylonitrile and 5 g of N,N-diethyl-2-acrylamide were added to 350 g of deionized water, stirred and mixed, potassium hydroxide was added to adjust the pH to 5, 0.8 g of initiator potassium persulfate was added, and heated to react at a temperature of 65° C. for 3 h. After the reaction was completed, the mixture was dried at a temperature of 85° C. for 10 h to obtain a multi-polymer;

[0067] (3) 5 g of the multi-polymer was added to 20 g of deionized water, the pH was adjusted to 8 using lithium hydroxide, and the mixture was stirred at a temperature of 80° C. for 2 h at a rate of 1800 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0068] Comparative Example 3

[0069] A method for preparing a water-soluble binder for lithium-ion batteries comprises the following steps:

[0070] (1) 10 g of carbon nanotubes were added to 550 g of anhydrous ethanol, stirred and mixed evenly, and then 15 g of γ-methacryloxypropyltrimethoxysilane was added and heated to react at a temperature of 70° C. for 18 h. After the reaction was completed, the mixture was cooled and filtered, and the residue was washed with ethanol and vacuum dried at 65° C. for 6 h to obtain olefin-modified carbon nanotubes;

[0071] (2) 3 g of acrylonitrile, 5 g of N,N-diethyl-2-acrylamide, and 3.5 g of acrylic acid were added to 350 g of deionized water, stirred and mixed, potassium hydroxide was added to adjust the pH to 5, 0.8 g of initiator potassium persulfate was added, and heated to react at a temperature of 65° C. for 3 h. After the reaction was completed, the mixture was dried at a temperature of 85° C. for 10 h to obtain a multi-polymer;

[0072] (3) 5 g of the multi-polymer was added to 20 g of deionized water, the pH was adjusted to 8 using lithium hydroxide, and the mixture was stirred at a temperature of 80° C. for 2 h at a rate of 1800 rpm to obtain a water-soluble binder for lithium-ion batteries.

[0073] The carbon nanotubes used in the embodiments and comparative examples were purchased from Beijing Dekedaojin Technology Co., Ltd., model CNT204 carbon nanotubes; the tannic acid used was tannic acid composed of resorcinol A rings; the isocyanate-terminated polyurethane used was prepared from isophorone diisocyanate and 2,2-dihydroxymethylpropionic acid to obtain an isocyanate-terminated linear hydrophilic prepolymer.

[0074] The water-soluble adhesive for lithium-ion batteries of the present invention can be used with positive and negative active materials to make electrode plates for lithium-ion batteries. The positive electrode can be lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, nickel cobalt aluminum and nickel cobalt manganese, and the negative electrode can be artificial graphite, natural graphite, activated carbon, or silicon-based composite negative electrode materials.

[0075] The lithium ion battery negative electrode was prepared by using the lithium ion battery water-soluble adhesive prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3; SiO x / C composite material is used as silicon-based negative electrode material, the mass fractions of silicon-based negative electrode material and lithium-ion battery water-soluble binder are 95.5wt% and 4.5wt%, respectively, and deionized water is added according to a total solid content of 45%, and the mixture is stirred and mixed to form negative electrode sheet slurries; the evenly dispersed slurry is passed through a 100-mesh sieve, and then coated on a 10μm thick copper foil as a current collector, dried at 120°C for 5min, and naturally cooled to room temperature, and rolled with a unit length load of 10×104N / m to obtain electrode sheets, and lithium-ion battery negative electrodes are obtained, corresponding to sample one, sample two, sample three, sample four, sample five, and sample six.

[0076] (1) Determination of peel strength: Sample 1, Sample 2, Sample 3, Sample 4, Sample 5, and Sample 6 were cut into strips of 20 cm × 2.5 cm, respectively, and a 1 mm thick steel plate was adhered to the current collector side with double-sided tape, and a transparent tape was attached to the coating layer side. The strips were peeled off in a 180° direction at a speed of 100 mm / min using a tensile testing machine, and the peel stress was measured. The test results are shown in Table 1.

[0077] Table 1 Peel strength test table

[0078]

[0079] According to the test results in Table 1, it can be seen that the water-soluble binder for lithium-ion batteries used in the negative electrode materials of lithium-ion batteries in Samples 4, 5, and 6 does not contain tannic acid. Compared with Samples 2 and 3, the peel strength is significantly reduced. The peel strength of the electrode sheet of the composite material with tannic acid added is significantly increased.

[0080] (2) Determination of Tg: The water-soluble binders for lithium-ion batteries in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were subjected to thermogravimetric analysis using a Mettler Toledo-DSC / TGA thermogravimetric analyzer. The test conditions were: 2 The test was carried out in an atmosphere with a heating rate of 10°C / min and a heating range of 20-800°C;

[0081] Table 2 Tg test table

[0082]

[0083] According to the test results in Table 2, it can be seen that in Example 1, Example 2, and Example 3, as the added carbon nanotubes, polymerized monomers, and isocyanate-terminated polyurethane contents increase, the thermal stability of the obtained lithium-ion battery water-soluble binder is improved, which is helpful for improving the cycle stability of the battery;

[0084] (3) Battery internal resistance test: Samples 1 to 6 were used as the negative electrode of the lithium-ion battery, and NCM523 nickel cobalt manganese oxide was used as the positive electrode of the lithium-ion battery. 1M LiPF 6Dissolved in a mixed solution of ethylene carbonate EC, ethyl methyl carbonate EMC, and diethyl carbonate DEC in a mass ratio of 3:2:5 as an electrolyte, and PE / PP material as a separator, P383450 lithium-ion batteries were made respectively, and recorded as sample 1, sample 2, sample 3, comparative sample 1, comparative sample 2, and comparative sample 3. At 25°C and in a voltage range of 2.5-4.2V, the lithium-ion batteries of sample 1, sample 2, sample 3, comparative sample 1, comparative sample 2, and comparative sample 3 were charged and discharged at 0.5C. The constant current method was used to test the first coulomb efficiency of the charge and discharge cycle and the coulomb efficiency and capacity retention rate after 50 cycles. After 50 cycles of charge and discharge, the battery internal resistance test results are shown in Table 3.

[0085] Table 3 Battery internal resistance test table

[0086]

[0087] According to the test results in Table 3, it can be seen that the film resistance of Sample 1, Sample 2 and Sample 3 is significantly reduced compared with Comparative Sample 1, Comparative Sample 2 and Comparative Sample 3. The carbon nanotubes have excellent conductive effect, indicating that the addition of carbon nanotubes can effectively reduce the internal resistance of the electrode sheet.

[0088] Sample 1, Sample 2, Sample 3, Comparative Sample 1, Comparative Sample 2, Comparative Sample 3, at 25°C, in the voltage range of 2.5-4.2V, the lithium ion batteries of Sample 1, Sample 2, Sample 3, Comparative Sample 1, Comparative Sample 2, Comparative Sample 3 were charged and discharged at 0.5C, and the constant current method was used to test the charge and discharge cycle. After 50 cycles of charge and discharge, the capacity retention rate was as follows Figure 2 shown.

[0089] Depend on Figure 2 It can be seen that the cyclic stability of samples 1, 2 and 3 is significantly improved after adding tannic acid and carbon nanotubes.

[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a water-soluble binder for lithium-ion batteries, characterized in that: The following steps are involved: Step 1, mixing anhydrous ethanol, carbon nanotubes and γ-methacryloxypropyltrimethoxysilane, heating to react, cooling, filtering, washing and drying after the reaction to obtain olefin-modified carbon nanotubes; Step 2: evenly mix deionized water and tannic acid, then add olefin-modified carbon nanotubes, acrylonitrile, N,N-diethyl-2-acrylamide, and acrylic acid, stir and mix, add potassium hydroxide to adjust the pH to 4-5, add an initiator, heat to react, and after the reaction is completed, dry to obtain a multi-polymer; Step 3: Evenly mix N,N-dimethylformamide, multi-polymer and stannous octoate, add isocyanate-terminated polyurethane in a nitrogen atmosphere, react during heating and refluxing, cool, precipitate, filter and dry after the reaction to obtain a cross-linked copolymer, add deionized water to the cross-linked copolymer, adjust the pH to 7-8 with lithium hydroxide, stir and mix to obtain a water-soluble binder for lithium ion batteries; In the step 2, the mass ratio of deionized water, tannic acid, olefin-modified carbon nanotubes, acrylonitrile, N,N-diethyl-2-acrylamide, acrylic acid, and initiator is 1800-3500:100:3-10:8-30:15-50:12-35:3-8; The reaction temperature in step 2 is 50-65°C and the reaction time is 3-8h; In the step 3, the mass ratio of N,N-dimethylformamide, multi-polymer, stannous octoate, and isocyanate-terminated polyurethane is 400-900:100:0.5-1:35-75; The reaction temperature in step 3 is 75-90° C., and the reaction time is 5-12 h.

2. The method according to claim 1, characterized in that: The initiator in step 2 includes one of potassium persulfate, benzoyl peroxide and ammonium persulfate.

3. The method according to claim 1, characterized in that In the step 3, the mass ratio of deionized water to the cross-linked copolymer is 100:10-25.

4. The method according to claim 1, characterized in that: In the step 3, the stirring temperature is 60-80° C., the stirring time is 2-5 h, and the stirring speed is 1200-1800 rpm.

5. A water-soluble binder for lithium-ion batteries prepared by the method for preparing a water-soluble binder for lithium-ion batteries according to any one of claims 1 to 4.

6. A lithium ion battery, characterized in that: The preparation of the lithium ion battery includes the water-soluble binder for lithium ion batteries according to claim 5.