Large field-induced strain leadless piezoelectric ceramic material, piezoelectric ceramic bending brake, preparation method and application
By introducing and controlling A-position defect dipoles in perovskite type piezoelectric ceramics, the pollution problem of lead-based materials to the environment is solved, and the large-field strain and displacement output of lead-free piezoelectric ceramics is achieved, providing A green alternative.
Patent Information
- Application Number
- CN202411158315.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
Existing lead-based piezoelectric ceramic materials are harmful to the environment and human health during the preparation, use and recycling process, and lead-free piezoelectric ceramic materials are difficult to replace traditional materials in terms of performance and production efficiency.
By introducing and controlling A-position defect dipoles in perovskite piezoelectric ceramic materials, the lead-free piezoelectric ceramic materials are prepared by actively introducing defect dipoles and forming them through casting Technology designs defective dipole concentration gradients to enhance the electrostatic displacement output of ceramics.
It achieves stable large-field strain and displacement output, solves the environmental pollution problem of lead-based materials, and significantly improves the performance and application potential of lead-free ceramics, providing a green and environmentally friendly alternative.
Smart Images

Figure CN119038994A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of piezoelectric ceramic materials and functional materials, and in particular to a lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles, a piezoelectric ceramic bending brake, and a preparation method and application thereof. Background Art
[0002] Piezoelectric brakes can realize the mutual conversion between electrical energy and mechanical energy, and ABO3 perovskite piezoelectric ceramic materials are favored by researchers because of their unique mechanical energy to electrical energy conversion function. Mechanoelectric conversion and spontaneous polarization make ferroelectric piezoelectric ceramics widely used in driving, precision displacement control and other fields. At present, the most widely used commercial piezoelectric ceramic actuator market is still lead zirconate titanate (PZT)-based ceramic materials. Commercial modified lead zirconate titanate ceramic materials can produce a strain of nearly 0.2% under a driving electric field of 20kV / cm, and their equivalent inverse piezoelectric coefficient is 1000pm / V. However, these are lead-based piezoelectric materials with a lead content of more than 60wt.%, and the lead element is extremely volatile during the sintering process. These lead-containing materials will cause serious harm to the ecological environment and the sustainable development of human society during the preparation, use and recycling process. Therefore, the development of environmentally friendly lead-free ferroelectric piezoelectric materials has become an important scientific frontier and technological competition focus internationally.
[0003] Lead-free ferroelectric material K 0.5 Na 0.5 As a perovskite ferroelectric material, NbO3 (abbreviated as KNN) not only has excellent ferroelectricity and piezoelectricity, good temperature stability and fatigue stability, but also can be prepared by traditional solid phase sintering method, and the preparation method is simple. It is one of the most promising piezoelectric ceramic materials that can replace PZT and be put into commercialization.
[0004] Through defect control engineering, field-induced strain comparable to that of lead zirconate titanate can be obtained in lead-free piezoelectric ceramics. However, the method of introducing defect dipoles in the potassium sodium niobate system to obtain large field-induced strain is mainly through the volatilization of potassium and sodium elements at the A position during sintering, which is extremely demanding on sintering conditions, and the content of defect dipoles is uncontrollable. Moreover, in mature production lines and large electro-induced displacement, it is difficult for lead-free ceramics to gain an advantage over lead-based ceramics when the performance is similar. Therefore, it is particularly important to develop a new method and strategy to improve the output of electro-induced displacement. Summary of the invention
[0005] In view of the limitations of the above-mentioned problems and the defects of the prior art, the main purpose of the present invention is to introduce A-site defect dipoles with the same direction as the spontaneous polarization into the orthorhombic perovskite piezoelectric ceramic material, so as to obtain stable defect dipoles with different concentrations, and provide a lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles, a piezoelectric ceramic bending brake, and a preparation method and application.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first aspect of the present invention provides a lead-free piezoelectric ceramic material with a large field-induced strain induced by actively introducing defect dipoles. The general formula of the lead-free piezoelectric ceramic is (1-xy)(K 0.5 Na 0.5 )Nb 1-x O3-x(BNbO3);
[0008] Wherein B is selected from Ca, Sr or Ba, the value range of x is 0.01 to 0.04, the value range of y is 0 to 0.02, and y can be equal to 0.
[0009] More preferably, the value range of y is 0.005 to 0.01.
[0010] The second aspect of the present invention provides a method for preparing the above-mentioned large field-induced strain lead-free piezoelectric ceramic material, wherein the preparation method is to actively introduce alkali metal A-site vacancies into the perovskite structure to obtain piezoelectric ceramic materials with defect dipoles of different concentrations. The specific preparation method comprises:
[0011] S1: According to the general formula (1-xy)(K 0.5 Na 0.5 )Nb 1-x O3-x(BNbO3), selecting raw materials including potassium salt, sodium salt, calcium salt, strontium carbonate salt, barium salt and niobium pentoxide for batching to obtain a first powder;
[0012] S2: adding anhydrous ethanol as a ball milling medium to the first powder for ball milling, and drying after ball milling to obtain a second powder;
[0013] S3: pre-sintering the second powder at 800-900° C. to form a third powder, adding 2wt%-8wt% of polyvinyl alcohol aqueous solution to the third powder for granulation to obtain powder;
[0014] S4: pressing the powder obtained in S3 into a green body, debinding it, and then sintering it at 1120-1150° C. to obtain a ceramic sheet;
[0015] S5: The ceramic sheet obtained in S4 is polished, coated with a silver electrode, and then polarized in silicone oil.
[0016] Furthermore, in S1, y is the content of different A-site vacancies introduced;
[0017] In S1, the raw materials specifically include potassium carbonate, sodium carbonate, calcium carbonate, strontium carbonate, barium carbonate, and niobium pentoxide.
[0018] Furthermore, in S3, the mass ratio of the polyvinyl alcohol aqueous solution to the ceramic powder is 0.05 to 0.1:1;
[0019] In S4, the pressing pressure is 180-200 MPa, the debinding time is 4-6 hours, the debinding temperature is 550°C, the sintering holding time is 4-6 hours, and an airtight alumina crucible with a threaded cover is used during sintering to suppress the volatilization of alkali metal elements.
[0020] Furthermore, in S5, the polarization temperature is 100-150° C., the polarization electric field strength is 2-4 kV / mm, and the polarization time is 5-30 min.
[0021] The third aspect of the present invention provides the use of the large field-induced strain lead-free piezoelectric ceramic material as described above in the preparation process of piezoelectric ceramic single chip drivers, piezoelectric tactile feedback, piezoelectric micro pumps, and piezoelectric fans.
[0022] A fourth aspect of the present invention provides a method for preparing a piezoelectric ceramic bending brake, comprising the following steps:
[0023] T1: pre-sintering the second powder as claimed in claim 2 at 800-900° C. to form a powder, and sieving it with a sieve to obtain a fine powder;
[0024] T2: Add a binder, a dispersant, a defoaming agent and an organic solvent to the fine powder, stir and mix them evenly into a slurry, and perform tape casting after vacuum defoaming the slurry to obtain a film tape;
[0025] T3: laminating the membrane strips of different components into a blank according to the defect concentration gradient, debinding, and then sintering at 1120-1150°C to obtain a ceramic sheet with a defect dipole concentration gradient;
[0026] T4: The ceramic sheet obtained in T3 is polished, coated with silver electrodes, and then polarized in silicone oil.
[0027] Further, in T1, the sieve is a 40-mesh sieve;
[0028] In T2, the binder is a mixture of polyvinyl butyral ester type 30 and type 60 (mass ratio 1:2), the dispersant is dioctyl phthalate, the defoaming agent is n-butanol, and the organic solvent is a mixture of anhydrous ethanol and n-butyl acetate;
[0029] The ratio of the binder, dispersant, defoamer and organic solvent is as follows: 1 part by weight of polyvinyl butyral ester 30 and 60 (1:2), 0.3 part by weight of dioctyl phthalate, 0.1 part by weight of n-butanol, 2 parts by weight of ethanol and 4.6 parts by weight of n-butyl acetate are added to 10 parts by weight of fine powder;
[0030] In T3, the lamination pressure is 180-220 MPa, the lamination temperature is 55-60°C, the debinding temperature is 600°C, and the debinding treatment time is 20 hours of heating and 2-4 hours of heat preservation;
[0031] In T4, the polarization temperature is 100-150°C, the polarization electric field strength is 2-4 kV / mm, and the polarization time is 5-30 min.
[0032] A fifth aspect of the present invention provides a piezoelectric ceramic bending brake obtained by the above-mentioned preparation method.
[0033] Compared with the prior art, the present invention has the following technical advantages:
[0034] 1) The present invention introduces a stable defect dipole in the potassium sodium niobate system through active design, and proposes a new strategy to obtain large field-induced displacement deformation in the potassium sodium niobate system by actively designing the concentration gradient through tape casting. Compared with the existing lead-containing piezoelectric ceramic actuators, the bending ceramic actuator of the potassium sodium niobate system has the characteristics of green and environmentally friendly, and its displacement output is greatly improved compared with the displacement of the traditional piezoelectric mode.
[0035] 2) It can effectively solve the environmental pollution problem caused by lead-based materials during the preparation process, and its large bending displacement can solve the large displacement that cannot be achieved based on the traditional piezoelectric effect, showing great potential in many application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is the X-ray diffraction pattern of KNBN0, KNBN0.5 and KNBN1 piezoelectric ceramics prepared in Examples 1-3.
[0037] Figure 2 It is the X-ray photoelectron spectrum of KNBN0, KNBN0.5 and KNBN1 piezoelectric ceramics prepared in Examples 1-3.
[0038] Figure 3 The bipolar equivalent strain-electric field (SE) curves of the KNBN0 piezoelectric ceramics prepared in Example 1 tested at thicknesses of 1000 μm, 500 μm, 300 μm and 150 μm, respectively.
[0039] Figure 4The bipolar equivalent strain-electric field (SE) curves of the KNBN0.5 piezoelectric ceramic prepared in Example 2 tested at thicknesses of 1000 μm, 500 μm, 300 μm and 150 μm, respectively.
[0040] Figure 5 The bipolar equivalent strain-electric field (SE) curves of the KNBN1 piezoelectric ceramic prepared in Example 3 tested at thicknesses of 1000 μm, 500 μm, 300 μm and 150 μm, respectively.
[0041] Figure 6 It is the cantilever tip displacement measured at 100, 200, 300, and 400 Vpp AC electric field and 70 Hz frequency for the KNBN-G ceramic with composition gradient prepared in Example 4 with a size of 20 mm (length) × 10 mm (width) × 0.15 mm (thickness).
[0042] Figure 7 (a) is the vibration acceleration of the piezoelectric tactile feedback element measured under 300V, 200Hz AC electric field excitation.
[0043] Figure 7 (b) is the measurement method of the vibration acceleration of the piezoelectric tactile feedback element.
[0044] Figure 8 This is a schematic diagram of the preparation process of the lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles in the present invention. DETAILED DESCRIPTION
[0045] In general, the present invention discloses a method for achieving large electro-induced strain by actively introducing defect dipoles and a general method for achieving large bending deformation by designing the concentration gradient of defect dipoles in a ceramic sheet by a tape casting method. 0.5 Na 0.5 )Nb 1-x Single-component lead-free piezoelectric ceramics and multi-component composition gradient lead-free piezoelectric ceramics of O3-x (BNbO3). B is selected from Ca, Sr or Ba, the value range of x is 0.01-0.04, and the value range of y is 0-0.02. The present invention realizes a new type of electro-bending deformation different from the traditional piezoelectric mode, thereby achieving a larger displacement output of the piezoelectric ceramic. The present invention makes up for the situation of insufficient displacement output in some current piezoelectric drive applications, and breaks through the problem of limited electro-strain value that often exists in materials in practical applications. Through the display of some applications, a new perspective is provided for the electro-bending deformation of lead-free piezoelectric ceramics, and also provides new ideas for the development of piezoelectric drives.
[0046] In specific implementation, the present invention actively introduces a large field-induced strain lead-free piezoelectric ceramic material induced by defect dipoles, and the general formula is (1-xy)(K 0.5 Na 0.5 )Nb 1-x O3-x(BNbO3), B is selected from Ca, Sr or Ba, the value range of x is 0.01 to 0.04, and the value range of y is 0 to 0.02.
[0047] In a specific implementation, the active introduction of defect dipole-induced large field-induced strain lead-free piezoelectric ceramic material is characterized by actively introducing alkali metal A-site vacancies in the perovskite structure and controlling the volatilization of the alkali metal element through the sintering process to obtain piezoelectric ceramic materials with different concentrations of defect dipoles, see Figure 8 , the preparation method comprises the following steps:
[0048] 1) According to the general formula (1-xy)(K 0.5 Na 0.5 )Nb 1-x O3-x(BNbO3) selects potassium carbonate, sodium carbonate, calcium carbonate, strontium carbonate, barium carbonate, niobium pentoxide and other raw materials for batching;
[0049] 2) adding anhydrous ethanol as a ball milling medium for ball milling, and drying after ball milling to obtain a mixed dry powder;
[0050] 3) pre-sintering the mixed dry powder at 800-900° C. to form a powder, adding 2wt%-8wt% of a polyvinyl alcohol aqueous solution to the powder for granulation to obtain a powder;
[0051] 4) Pressing the powder into a green body, debinding the green body at 550°C, and then sintering the green body at 1120-1150°C to obtain a ceramic sheet;
[0052] 5) The ceramic sheet is polished, coated with silver electrodes, and then polarized in silicone oil.
[0053] During specific implementation, in step 1), y is the content of different A vacancies introduced.
[0054] In the specific implementation, in step 3), the mass ratio of the polyvinyl alcohol aqueous solution to the ceramic powder is 0.05 to 0.1:1.
[0055] In the specific implementation, the pressing pressure in step 4) is 180-200 MPa, the debinding time is 4-6 hours, the sintering and heat preservation time is 4-6 hours, and an alumina crucible with a threaded cover with good airtightness is used for sintering to control the volatilization of alkali metal elements.
[0056] In the specific implementation, in step 5), the polarization temperature is 100-150° C., the polarization electric field strength is 2-4 kV / mm, and the polarization time is 5-30 min.
[0057] In a specific implementation, based on the active introduction of piezoelectric ceramic components with defect dipoles of different concentrations, a concentration gradient of defect dipoles is constructed by a casting method to produce a piezoelectric ceramic bending brake. The method includes the following steps:
[0058] a) pre-sintering the mixed dry powder in step 3) at 800-900° C. to form a powder, and sieving it with a sieve to obtain a fine powder;
[0059] b) adding a binder, a dispersant, a defoaming agent and an organic solvent to the fine powder, stirring and mixing them uniformly to form a slurry, and performing tape casting after vacuum defoaming the slurry to obtain a film tape;
[0060] c) laminating the membrane strips of different components into a blank according to the defect concentration gradient, performing a binder removal treatment at 600° C., and then sintering at 1120-1150° C. to obtain a ceramic sheet with a defect dipole concentration gradient;
[0061] d) The ceramic wafer is polished, coated with silver electrodes, and then polarized in silicone oil.
[0062] During specific implementation, in step a), the sieve is a 40-mesh sieve.
[0063] In the specific implementation, in step b), the binder is a mixture of polyvinyl butyral ester type 30 and type 60, the dispersant is dioctyl phthalate, the defoaming agent is n-butanol, and the organic solvent is a mixture of anhydrous ethanol and n-butyl acetate.
[0064] In the specific implementation, in step c), the lamination pressure is 180-220 MPa, the lamination temperature is 55-60° C., and the debinding treatment time is 20 hours of heating and then 2-4 hours of heat preservation.
[0065] In the specific implementation, in step d), the polarization temperature is 100-150° C., the polarization electric field strength is 2-4 kV / mm, and the polarization time is 5-30 min.
[0066] The present invention provides the application of the large field-induced deformation lead-free piezoelectric ceramic material induced by the defect dipole concentration gradient in piezoelectric elements, including piezoelectric ceramic single-chip drivers, piezoelectric tactile feedback, piezoelectric micropumps, piezoelectric fans, etc.
[0067] In specific implementation, the single-piece piezoelectric ceramic sheet (20mm×10mm×0.15mm) with a defect dipole concentration gradient in the present invention can produce a bidirectional displacement of the cantilever beam tip exceeding ±1500 microns under an AC electric field of 400Vpp; the piezoelectric tactile feedback component made by tightly combining the piezoelectric ceramic single piece with a metal sheet can produce an acceleration of 2.0G under a load of 20g weight; the working mode of the piezoelectric ceramic can also be applied to piezoelectric micropumps, and its new bending drive mode shows a very broad application scenario in the application of piezoelectric elements.
[0068] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Any features such as preparation means, materials, structures or composition ratios not clearly described in this technical solution are regarded as common technical features disclosed in the prior art.
[0069] Example 1
[0070] The preparation composition is 0.98 (K 0.5 Na 0.5 )Nb 0.98 The preparation method of potassium sodium niobate-based piezoelectric ceramics of O3-0.02(SrNbO3) (abbreviated as KNBN0) and testing its electrical properties includes the following steps:
[0071] The first step is to follow the general formula 0.98 (K 0.5 Na 0.5 )Nb 0.98 O3-0.02(SrNbO3) Weigh high-purity (purity not less than 98%) Na2CO3, K2CO3, Nb2O5, SrCO3 powder raw materials and ball-mill them in anhydrous ethanol medium for 24h;
[0072] Step 2: Dry the dispersion obtained in the first step, and calcine the obtained powder in air at 850°C for 6h;
[0073] Step 3: ball mill the powder obtained in step 2 in anhydrous ethanol medium for 24 hours;
[0074] Step 4: Dry the dispersion obtained in step 3, cold-press the obtained powder, and sinter it in air at 1120° C. for 4 hours. During sintering, use an alumina crucible with a threaded lid and good airtightness to control the volatilization of alkali metal elements.
[0075] Step 5: Polish the ceramic sheet, apply silver electrodes, and then polarize in silicone oil at a temperature of 120°C, a polarization electric field strength of 3 kV / mm, and a polarization time of 30 min.
[0076] Example 2
[0077] The preparation composition is 0.955 (K 0.5 Na0.5 )Nb 0.98 The preparation method of this embodiment is similar to that of embodiment 1, except that in the first step, 0.955 (K 0.5 Na 0.5 )Nb 0.98 The chemical formula of O3-0.02 (SrNbO3) is used to weigh the raw materials. During the batching process, 0.5% of the A-site defect dipole is introduced, that is, y is 0.005.
[0078] Example 3
[0079] The preparation composition is 0.95 (K 0.5 Na 0.5 )Nb 0.98 The preparation method of this embodiment is similar to that of embodiment 1, except that in the first step, 0.95 (K 0.5 Na 0.5 )Nb 0.98 The chemical formula of O3-0.02 (SrNbO3) is as follows: the raw materials are weighed, and 1% of the A-site defect dipole is introduced into the ingredients, that is, y is 0.01.
[0080] Example 4
[0081] A concentration gradient KNN-based ceramic (abbreviated as KNBN-G) composed of KNBN0 and KNBN1 was prepared, and its electrical properties were tested. The preparation method includes the following steps:
[0082] The first step is to follow the general formula 0.98 (K 0.5 Na 0.5 )Nb 0.98 O3-0.02(CaNbO3) and 0.95(K 0.5 Na 0.5 )Nb 0.98 O3-0.02(SrNbO3) Weigh high-purity (purity not less than 98%) Na2CO3, K2CO3, Nb2O5, CaCO3 powder raw materials and ball-mill them in anhydrous ethanol medium for 24h;
[0083] Step 2: adding anhydrous ethanol as a ball milling medium for ball milling, and drying after ball milling to obtain a mixed dry powder;
[0084] The third step is to pre-sinter the mixed dry powder at 900°C to form a powder, and then sieve the powder with a 40-mesh screen to obtain a fine powder;
[0085] Step 4: Add 1g of polyvinyl butyral ester type 30 and type 60 (1:2), 0.3g of dioctyl phthalate, 0.1g of n-butanol, 2g of ethanol and 4.6g of n-butyl acetate to 10g of fine powder and stir to mix evenly into slurry, vacuum degas the slurry and perform tape casting to obtain a 50μm thick film tape;
[0086] Step 5: Laminate two layers of KNBN0 membrane tape and two layers of KNBN1 membrane tape into a blank according to a concentration gradient, perform a binder removal treatment at 600°C, and then sinter at 1120°C to obtain a ceramic sheet.
[0087] Verification Example 1
[0088] The effects that can be obtained by the above embodiment will be described below in conjunction with specific experiments.
[0089] 1. X-ray diffraction pattern
[0090] Figure 1 X-ray diffraction patterns of KNBN0, KNBN0.5 and KNBN1 piezoelectric ceramics prepared in Examples 1-3 of the present invention. It can be found from the patterns that the piezoelectric ceramics of different compositions prepared in the technical solution of the present invention are all perovskite structures at room temperature without impurities. The XRD patterns of KNBN0.5 and KNBN1 piezoelectric ceramics are very similar to the KNN standard patterns of the orthorhombic phase Amm2 space group, indicating that KNBN0.5 and KNBN1 piezoelectric ceramics exhibit orthorhombic phase structures at room temperature. In the KNBN0 component where defects are not actively introduced, the diffraction peaks gradually become more symmetrical, and the peak separation phenomenon is not obvious, indicating that the phase structure of the piezoelectric ceramics changes to a pseudocubic structure. It can also be seen from this that the active introduction of defects may lead to a decrease in lattice symmetry.
[0091] 2. X-ray Photoelectron Spectroscopy
[0092] Figure 2 X-ray photoelectron spectra of KNBN0, KNBN0.5 and KNBN1 piezoelectric ceramics prepared for inventive embodiments 1-3. It can be found from the spectrum that as the content of defect dipoles actively introduced by KNBN0, KNBN0.5 and KNBN1 gradually increases, the relative intensity of oxygen vacancies shows a trend of gradually increasing. Since the formation of defect dipoles requires an oxygen vacancy with a +2 valence and two A-position vacancies with a -1 valence, the relative content of oxygen vacancies can reflect the content of A-position vacancies and defect dipoles from the side. Therefore, with the increase of actively introduced A-position vacancies, the oxygen vacancy content gradually increases. This also illustrates the successful introduction of defect dipoles and the increase in the content of defect dipoles.
[0093] 3. Electrical performance test
[0094] Test method: The piezoelectric ceramic sheets prepared in Examples 1-3 were respectively ground to 1000 μm, 500 μm, 300 μm and 150 μm. Using an aixACCT TF1000 ferroelectric properties tester, the samples were clamped in upper and lower clamps with an area larger than their own size under 30 kV / cm, 10 Hz bipolar or monopolar triangular wave excitation, and the equivalent strain (displacement / thickness)-electric field (SE) curve of the piezoelectric ceramics was tested. During the test, the samples were completely immersed in silicone oil.
[0095] like Figure 3 Shown are the strain-electric field (SE) curves of the KNBN0 piezoelectric ceramics prepared in Example 1 at different thicknesses. It can be seen from the SE curve that as the sample thickness decreases, the bidirectional strain curve measured under the same electric field conditions changes from a completely symmetrical butterfly curve at 1000 μm to a completely asymmetric strain curve with defect dipole contribution characteristics at 150 μm. This reflects that as the thickness decreases, the contribution of defect dipoles to the electrostrain under stretching in a positive electric field and contraction in a negative electric field becomes more and more significant. Since the KNBN0 sample does not actively introduce defects, the defect dipoles come from the volatilization of a small amount of unavoidable alkali metal elements during the sintering process.
[0096] like Figure 4 Shown are the strain-electric field (SE) curves of the KNBN0.5 piezoelectric ceramics prepared in Example 2 at different thicknesses. It can be seen from the SE curve that as the thickness of the sample decreases, the bidirectional strain curve measured under the same electric field conditions also shows that the contribution of the defect dipole to the strain gradually increases. Compared with the KNBN0 sample without actively introducing defects, KNBN0.5 actively introduces 0.5% of defect dipoles. Due to the increase in the content of defect dipoles, the sample shows a completely asymmetric strain curve at 300μm, and compared with the KNBN0 sample at the same thickness, the strain value of the KNBN0.5 sample increases due to the increase in the content of defect dipoles, which proves the active introduction of defect dipoles and the contribution of defect dipoles to strain.
[0097] like Figure 5 The following are the strain-electric field (SE) curves of the KNBN1 piezoelectric ceramics prepared in Example 3 at different thicknesses. It can be seen from the SE curve that, similar to the test results of KNBN0.5, the KNBN1 sample actively introduced 1% of defect dipoles. Therefore, due to the higher content of defect dipoles, the sample showed a completely asymmetric strain curve at 500 μm, and compared with the KNBN0 and KNBN0.5 samples at the same thickness, the strain value of the KNBN1 sample increased due to the increase in the content of defect dipoles, and a large negative strain appeared, which further proved the active introduction of defect dipoles and the contribution of defect dipoles to strain.
[0098] The specific test results of each embodiment are as follows:
[0099] The electrical properties of the piezoelectric ceramics prepared in Example 1 are as follows: the strain value under zero field in the SE curve is determined as 0, and the maximum equivalent strain under 30kV / cm, 1000μm bipolar excitation voltage is about 0.042%; the maximum equivalent strain under 30kV / cm, 500μm bipolar excitation voltage is about 0.048%; the maximum equivalent strain under 30kV / cm, 300μm bipolar excitation voltage is about 0.098%; the maximum equivalent strain under 30kV / cm, 150μm bipolar excitation voltage is about 0.27%. The quotient Smax / Emax of the maximum equivalent strain and the maximum electric field strength is used to evaluate the electrodisplacement output performance, which is about 900pm / V under 30kV / cm, 150μm bipolar excitation.
[0100] The electrical properties of the piezoelectric ceramics prepared in Example 2 are as follows: the strain value under zero field in the SE curve is determined as 0, and the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 1000μm is about 0.076%; the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 500μm is about 0.082%; the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 300μm is about 0.17%; the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 150μm is about 0.45%. The quotient Smax / Emax of the maximum equivalent strain and the maximum electric field strength is used to evaluate the electrodisplacement output performance, which is about 1500pm / V under bipolar excitation of 30kV / cm, 150μm.
[0101] The electrical properties of the piezoelectric ceramics prepared in Example 3 are as follows: the strain value under zero field in the SE curve is determined as 0, and the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 1000μm is about 0.071%; the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 500μm is about 0.1%; the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 300μm is about 0.22%; the maximum equivalent strain under bipolar excitation voltage of 30kV / cm, 150μm is about 0.66%. The quotient Smax / Emax of the maximum equivalent strain and the maximum electric field strength is used to evaluate the electrodisplacement output performance, which is about 2200pm / V under bipolar excitation of 30kV / cm, 150μm.
[0102] 4. Electrodeformation test
[0103] Taking the multi-component concentration gradient ceramic KNBN-G prepared in Example 4 as an example, a cantilever beam tip displacement test was performed using a Doppler laser vibrometer under AC excitation of ±150 V, 70 Hz.
[0104] Figure 6 This is the vibration deformation test result of KNBN-G. The size of the sample is 20mm (length) × 10mm (width) × 0.15mm (thickness). It is fixed in a cantilever beam manner. The cantilever beam extends 18mm and the displacement of the tip of the cantilever beam is tested. It can be seen that the sample has obvious bending deformation visible to the naked eye under 70Hz (resonance frequency) and ±200V AC electric field, and the amplitude of the displacement difference can reach 3000μm. The amplitudes under 70Hz (resonance frequency) ±50V, ±100V, and ±200V AC electric fields are ±150μm, ±470μm, and ±900μm, respectively.
[0105] 5. Piezoelectric tactile feedback element performance test
[0106] Preparation of piezoelectric tactile feedback element: The 20×10×0.25 mm piezoelectric ceramic KNBN-G prepared in Example 4 was coated with silver on both sides and bonded to a 42Fe-Ni alloy plate with dimensions of 30×15×0.1 mm using epoxy conductive silver glue, and electrodes were led out. A 300 V, 200 Hz AC electric field excitation drive test was performed.
[0107] Figure 7 (a) is the vibration acceleration of the piezoelectric tactile feedback element measured under 300V, 200Hz AC electric field excitation. It can be seen that the vibration acceleration of the sample is 3.0G under no-load condition, and the vibration acceleration under 20g and 100g weights is 2.0G and 0.35G respectively. Vibration acceleration is an important indicator of piezoelectric tactile feedback. The vibration acceleration of the sample under 20g and 100g loads shows the application prospects of this material in the field of piezoelectric tactile feedback.
[0108] Figure 7 (b) is the vibration acceleration measurement method. A standard piezoelectric accelerometer with a sensitivity of 10mV / g is used to measure vibration acceleration. The piezoelectric accelerometer outputs a voltage signal, and acceleration G = voltage / sensitivity.
[0109] In summary, the present invention realizes large electro-induced strain at different defect dipole concentrations by actively introducing defect dipoles, and realizes a method of designing a defect dipole concentration gradient in a ceramic sheet by a tape casting method, and realizes large bending deformation of a single ceramic sheet visible to the naked eye. The present invention breaks through the problem of limited electro-induced strain value that often exists in materials in practical applications. And through the demonstration of some applications, it provides a new perspective for the electro-induced bending deformation of lead-free piezoelectric ceramics, and also provides new ideas for the development of piezoelectric actuators.
[0110] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A lead-free piezoelectric ceramic material with large field-induced strain induced by active defect dipoles, characterized in that: The general formula of the lead-free piezoelectric ceramic is (1-xy)(K 0.5 Na 0.5 )Nb 1-x O3-x(BNbO3); Wherein B is selected from Ca, Sr or Ba, the value range of x is 0.01 to 0.04, and the value range of y is 0 to 0.
02.
2. A method for preparing a lead-free piezoelectric ceramic material with large field-induced strain as claimed in claim 1, characterized in that: The preparation method is to actively introduce alkali metal A-site vacancies into the perovskite structure to obtain piezoelectric ceramic materials with defect dipoles of different concentrations. The specific preparation method includes: S1: According to the general formula (1-xy)(K 0.5 Na 0.5 )Nb 1-x O3-x(BNbO3), selecting raw materials including potassium salt, sodium salt, calcium salt, strontium carbonate salt, barium salt and niobium pentoxide for batching to obtain a first powder; S2: adding anhydrous ethanol as a ball milling medium to the first powder for ball milling, and drying after ball milling to obtain a second powder; S3: pre-sintering the second powder at 800-900° C. to form a third powder, adding 2wt%-8wt% of polyvinyl alcohol aqueous solution to the third powder for granulation to obtain powder; S4: pressing the powder obtained in S3 into a green body, debinding it, and then sintering it at 1120-1150° C. to obtain a ceramic sheet; S5: The ceramic sheet obtained in S4 is polished, coated with a silver electrode, and then polarized in silicone oil.
3. The method for preparing a lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles according to claim 2, characterized in that: In S1, y is the content of different A-site vacancies introduced; In S1, the raw materials specifically include potassium carbonate, sodium carbonate, calcium carbonate, strontium carbonate, barium carbonate, and niobium pentoxide.
4. The method for preparing a lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles according to claim 2, characterized in that: In S3, the mass ratio of the polyvinyl alcohol aqueous solution to the ceramic powder is 0.05-0.1:
1.
5. The method for preparing a lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles according to claim 2, characterized in that: In S4, the pressing pressure is 180-200 MPa, the debinding time is 4-6 hours, the debinding temperature is 550°C, the sintering holding time is 4-6 hours, and an airtight alumina crucible with a threaded cover is used during sintering to suppress the volatilization of alkali metal elements.
6. The method for preparing a lead-free piezoelectric ceramic material with large field-induced strain induced by actively introducing defect dipoles according to claim 2, characterized in that: In S5, the polarization temperature is 100-150° C., the polarization electric field strength is 2-4 kV / mm, and the polarization time is 5-30 min.
7. An application of the large field-induced strain lead-free piezoelectric ceramic material as claimed in claim 1 in the preparation process of piezoelectric ceramic single chip driver, piezoelectric tactile feedback, piezoelectric micro pump and piezoelectric fan.
8. A method for preparing a piezoelectric ceramic bending brake, characterized in that: The following steps are involved: T1: pre-sintering the second powder as claimed in claim 2 at 800-900° C. to form a powder, and sieving it with a sieve to obtain a fine powder; T2: Add a binder, a dispersant, a defoaming agent and an organic solvent to the fine powder, stir and mix them evenly into a slurry, and perform tape casting after vacuum defoaming the slurry to obtain a film tape; T3: laminating the membrane strips of different components into a blank according to the defect concentration gradient, debinding, and then sintering at 1120-1150°C to obtain a ceramic sheet with a defect dipole concentration gradient; T4: The ceramic sheet obtained in T3 is polished, coated with silver electrodes, and then polarized in silicone oil.
9. The method for preparing a piezoelectric ceramic bending brake according to claim 8, characterized in that: In T1, the sieve is a 40-mesh sieve; In T2, the binder is a mixture of polyvinyl butyral ester type 30 and type 60, the dispersant is dioctyl phthalate, the defoaming agent is n-butanol, and the organic solvent is a mixture of anhydrous ethanol and n-butyl acetate; In T3, the lamination pressure is 180-220MPa, the lamination temperature is 55-60℃, the debinding temperature is 600℃, and the debinding treatment time is 20h heating and 2-4h insulation; In T4, the polarization temperature is 100-150°C, the polarization electric field strength is 2-4 kV / mm, and the polarization time is 5-30 min.
10. A piezoelectric ceramic bending brake obtained by the preparation method according to claim 8 or 9.
Citation Information
Patent Citations
Lead-free piezoelectric ceramic material and preparation method thereof
CN116283273A
Lead-free piezoelectric fiber composite material driver for active control of cantilever beam vibration and preparation method and application of lead-free piezoelectric fiber composite material driver
CN116404899A
Ultrasonic motor with annular piezoelectric vibrator for optical apparatus
EP3174191A1
Method for preparing nanotubes of piezoelectric material and nanotubes of piezoelectric material obtained thereby
US20100102033A1