Economical flux-cored wire for duplex stainless steel and manufacturing method thereof
By reasonably preparing alumina, metal chromium and other constituent materials in flux-core welding wire, the problems of full-position welding and low-temperature toughness in welding economical duplex stainless steel are solved, and the efficient molding and good mechanical properties of the weld are achieved.
Patent Information
- Application Number
- CN202411170442.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult to achieve full-position welding in the welding economical duplex stainless steel 2101, and the problems of poor slag removal on the surface of the weld and poor low-temperature toughness on the weld metal.
It uses high-purity spherical magnesium magnesium, metal chromium, nickel powder, zircon sand, bismuth oxide, ice crystal, aluminum powder, rutile, quartz sand, titanium iron, electrolytic manganese, ferrochromium nitride, potassium titanate, nanocrystalline high-purity spherical magnesium Flux-core welding wire composed of powder and Teflon, through reasonable formulation and manufacturing methods, ensure that the welding wire has good welding process and low-temperature impact toughness.
The welding process has been optimized, the weld is beautifully formed and easy to remove slag. The impact power of the weld metal at -40℃ can reach more than 47J. The welding performance complies with the EN IS017633-A-T237N L P C 1 standard, tensile strength and elongation. Good, strong pitting resistance.
Smart Images

Figure BDA0005009112410000061 
Figure BDA0005009112410000071 
Figure BDA0005009112410000072
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stainless steel welding, and in particular provides an economical flux-cored welding wire for duplex stainless steel and a manufacturing method thereof, which is suitable for all-position welding of economical duplex stainless steel DSS2101. Background Art
[0002] Economical duplex stainless steel 2101 (Duplex Stainless Steel 2101) is a ferrite-austenite duplex stainless steel. It is a duplex stainless steel with reduced content of precious metals such as nickel and molybdenum. It has a lower production cost and price on the basis of maintaining the excellent performance of duplex stainless steel, so as to improve its competitiveness with other general stainless steels. Economical duplex stainless steel 2101 has the advantages of both ferritic stainless steel and austenitic stainless steel, and has the following performance characteristics: ① Good resistance to chloride stress corrosion, which can effectively resist stress corrosion cracking under certain environments; ② Good resistance to pitting corrosion; ③ Good comprehensive mechanical properties and high yield strength, which is usually twice that of ordinary austenitic stainless steel; ④ Good weldability and low tendency to thermal cracking. Generally, no preheating is required before welding, and no heat treatment is required after welding. It can be welded with dissimilar austenitic stainless steel or carbon steel; ⑤ Compared with austenitic stainless steel, it has a large thermal conductivity and a small linear expansion coefficient. 2101 duplex stainless steel has high strength and good corrosion resistance. Its yield strength is twice that of traditional austenitic stainless steel. It also has good resistance to stress corrosion cracking and pitting corrosion. Due to its excellent performance, economical duplex stainless steel 2101 is widely used in petrochemical, marine engineering, papermaking, food processing and other fields, such as manufacturing pipelines, valves, heat exchangers, storage tanks and other equipment.
[0003] Therefore, the present invention proposes an economical flux-cored welding wire for duplex stainless steel and a manufacturing method thereof, which is of great significance for restricting the problems existing in welding economical duplex stainless steel 2101. Summary of the invention
[0004] In order to overcome the technical defects of existing flux-cored welding wires, such as difficulty in achieving all-position welding, poor slag removal on the weld surface and generally low low-temperature toughness of the weld metal, the present invention provides an economical flux-cored welding wire for duplex stainless steel, which has the characteristics of good all-position welding process, easy slag removal, high low-temperature impact toughness, etc.
[0005] In order to achieve the purpose of the present invention, the technical solution adopted is:
[0006] An economical flux-cored welding wire for duplex stainless steel, the flux-cored welding wire is composed of a steel strip outer skin and a flux core, and the raw material of the flux core is calculated by percentage to the total ratio of the welding wire, including the following components:
[0007] Alumina 0.05-0.15%;
[0008] Metal chromium 1.0-1.5%;
[0009] Nickel powder 0.15-0.4%;
[0010] Zircon sand 0.08~0.24%;
[0011] Bismuth oxide 0.01~0.03%;
[0012] Cryolite 0.25~0.055%;
[0013] Aluminum powder 0.025~0.045%;
[0014] Rutile 0.9-1.2%;
[0015] Quartz sand 0.025~0.4%;
[0016] Ferrotitanium 0.04-0.12%;
[0017] Electrolytic manganese 0.08~0.24%;
[0018] Ferrochromium nitride 0.15-0.24%;
[0019] Potassium titanate 0.1-0.3%;
[0020] Nanocrystalline high-purity spherical magnesium powder 0.04-0.12%;
[0021] Teflon 0.01-0.03%, the balance is iron powder.
[0022] In a preferred embodiment of the present invention, the iron powder is reduced iron powder or atomized iron powder.
[0023] In a preferred embodiment of the present invention, except for Teflon, the particle size range of each component of the drug core is -80 mesh to +160 mesh.
[0024] In a preferred embodiment of the present invention, the particle size of the Teflon is below -220 mesh to +375 mesh, and the friction coefficient is 0.03-0.15.
[0025] In a preferred embodiment of the present invention, the finished product specification of the flux-cored welding wire is 0.8mm-1.2mm.
[0026] The beneficial effects of the present invention are:
[0027] 1. The present invention reasonably designs the ratio of various powders in the formula, so that the welding wire of the present invention has good welding processability, is suitable for all-position welding, has beautiful weld formation, is easy to remove slag, and can be suitable for welding of economical duplex stainless steel 2101 steel base material.
[0028] 2. The magnesium powder added in the present invention is nanocrystalline high-purity spherical magnesium powder. Compared with traditional magnesium powder, this magnesium powder is a high-purity spherical magnesium alloy powder with a nanocrystalline structure, which has the characteristics of higher purity, more uniform particle size, and higher surface activity. It has a good effect on improving the low-temperature impact toughness of the weld. The proportion added in the present invention can make the impact energy of the weld metal at -40°C reach more than 47J.
[0029] 3. The Teflon powder added in the present invention has a particle size of -220 mesh to +375 mesh and has a very low friction coefficient of 0.03-0.15. It has a good lubricating effect and can be used as a solid lubricant to make the powder more fluid and the welding process more optimal, and can solve the slag removal problem of stainless steel flux-cored welding wire caused by uneven powder.
[0030] 4. Slag-forming agents and arc stabilizers such as alumina, rutile, potassium titanate, and quartz sand are added to the flux core, so it has good welding processability, soft arc, and small welding spatter. It is suitable for economical duplex stainless steel DSS2101 all-position welding. Its chemical composition meets the EN IS017633-A-T237N LPC 1 standard. At the same time, the weld has excellent mechanical properties, good impact resistance, and strong pitting resistance. Its tensile strength Rm ≥ 570MPa, ReL ≥ 450MPa, elongation A ≥ 20%, and pitting resistance equivalent PREN index ≥ 26.
[0031] The present invention also discloses an economical flux-cored welding wire for duplex stainless steel and a manufacturing method thereof, comprising the following steps:
[0032] (1) Raw material processing process:
[0033] The added rutile, quartz sand and zircon sand are calcined in a high temperature furnace at 900℃-1000℃ in trays, with the material placed on each tray not exceeding 50mm, and kept warm for 2h;
[0034] The added alumina, cryolite and potassium titanate are calcined in a high temperature furnace at 450℃-550℃ in trays, with the material placed on each tray not exceeding 50mm, and kept warm for 2h;
[0035] Prepare the raw material components of the core according to the proportion and bake at 220℃-270℃, keep warm for 2-3h, and stir the powder after it cools to no higher than 60℃ for 30-60min;
[0036] (2) Powder filling process: After the steel strip is formed into a U-shaped groove by a roller, it is filled with 25%-27% powder, and the seam is overlapped during the seam joining process;
[0037] (3) Fine drawing process and layer winding process: A calibrator is installed in the fine drawing process and the layer winding process.
[0038] The manufacturing method of the present invention has the following beneficial effects:
[0039] 1. The installation of a calibrator can effectively avoid the poor linearity of stainless steel flux-cored welding wire due to the high filling rate of steel strip and powder, thus affecting the welding quality.
[0040] 2. The formula of the flux-cored welding wire of the present invention and the special manufacturing process can make the linearity of the finished flux-cored welding wire meet the requirements of rebound>1000mmm and warpage<5mm. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the scope of the present invention.
[0042] The alumina in the present invention forms slag together with other mineral components to protect the welding pool. The melting point of alumina is about 2054°C, which has the effect of improving the vertical welding performance. In addition, it also helps to control the proportion of each phase in the weld, cooperates with other alloy elements, and produces a certain proportion of ferrite and austenite in the weld, thereby ensuring the performance of the weld.
[0043] The melting point of the nickel powder in the present invention is about 1452°C. It has a lower affinity with oxygen than iron, is not easily oxidized during welding, and has a high transition coefficient. Nickel is an austenite-forming element, which can change the crystal structure of steel and improve some properties of stainless steel, such as plasticity, weldability and toughness.
[0044] The electrolytic manganese in the present invention is rationally compounded in a certain proportion to play the role of deoxidation, desulfurization and improving the strength of the weld. Manganese is a weak austenite-forming element and can increase the solubility of nitrogen in steel to a certain extent. Manganese and nitrogen are often added in combination to replace expensive and scarce nickel in steel, which can not only replace nickel in order to obtain austenite structure, but also increase the nitrogen content in steel, stabilize or control the appropriate phase ratio, improve the performance of steel, and save nickel at the same time.
[0045] In the present invention, the metal chromium combines with oxygen to form a corrosion-resistant Cr2O3 passivation film, which is one of the basic elements for stainless steel to maintain corrosion resistance. Increasing the chromium content can significantly improve the corrosion resistance of stainless steel to oxidizing acids, and also improve the pitting corrosion resistance. Promote ferrite formation: Chromium is a ferrite-forming element. Increasing the chromium content in Fe-Cr-C or Fe-Cr-Ni-C alloys will promote the formation and retention of ferrite. Strengthen carbide: It is a very strong carbide-forming element. Common chromium-rich carbides are M 23C6, where M is mainly chromium, but sometimes also some iron and molybdenum. Cr7C3 type carbides may also be formed in duplex stainless steel, as well as other complex carbides and carbonitrides, such as M 23 CN6, etc. Solid solution strengthening to a certain extent: Since chromium can be used as a replacement atom in both body-centered cubic (BCC) and face-centered cubic (FCC) lattices, chromium can play a role of solid solution strengthening to a certain extent from the perspective of mechanical properties.
[0046] The titanium iron mentioned in the present invention mainly provides Ti element, which has a strong binding force with oxygen. Adding a certain amount of titanium iron into the flux core can play a deoxidation role, reduce the oxygen content of the weld metal, and promote the refinement of the weld metal.
[0047] The rutile in the present invention mainly plays the role of slag formation and arc stabilization during the welding process. The rutile has good thermal slag removal performance, stable arc, calm molten pool, good directional welding and excellent weld formation.
[0048] The Teflon mentioned in the present invention has a very low friction coefficient and good lubrication effect, and can be used as a solid lubricant. The addition of Teflon makes it easier to even out the powders in the core and the filling is more stable. After the molding is completed, the filling rate fluctuation is less than or equal to 0.35%. When the carbon dioxide gas shielded welding method is used for welding, the molding effect is better during the welding process and the mechanical properties are more stable.
[0049] The magnesium powder added in the present invention is nanocrystalline high-purity spherical magnesium powder, which is formed by various processing steps under the protection of inert gas using centrifugal atomization technology. Compared with the existing magnesium powder for flux-cored welding wire, it has high bulk density, good fluidity, small specific surface area, lower impurity content, easier to be evenly distributed in the flux core, good deoxidation effect, and stable mechanical properties of the weld metal.
[0050] The iron powder mentioned in the present invention can improve the welding deposition efficiency and adjust the proportion of alloy elements in the weld metal. The iron powder can be reduced iron powder or atomized iron powder.
[0051] The following is further described in conjunction with the embodiments of the present invention:
[0052] The required rutile, quartz sand and zircon sand are pre-calcined in a high-temperature furnace at 900℃-1000℃ in separate plates, with the material placed on each plate not exceeding 50mm, and kept warm for 2 hours.
[0053] The added alumina, cryolite and potassium titanate are calcined in a high temperature furnace at 450°C-550°C in plates, with the material placed in each plate not exceeding 50mm, and kept warm for 2 hours.
[0054] The particle size range of the powder of each component (except Teflon) of the core of the flux-cored welding wire is -80 mesh to +160 mesh. The Teflon powder is first sieved with a 220-mesh screen, and then a 375-mesh screen is used to remove the ultrafine powder. The powder is prepared according to the embodiment in Table 1.
[0055] Table 1 shows the core ratios in Examples 1-4:
[0056]
[0057]
[0058] The composite powder prepared in the above embodiment is baked at 220℃-270℃, kept warm for 2-3h, and stirred when the powder is cooled to no higher than 60℃ for 30-60min. The loose density and fluidity of the composite powder are tested using a Hall flow meter. The outer skin of the welding wire steel strip is a 304L steel strip with a specification of 0.4×10mm (chemical composition is shown in Table 2 below). The powder is loaded into the steel strip at a filling rate of 25%-27% through the molding process. When the molding is offline, five 20-30cm welding wires are cut to test the filling rate (three repeated tests).
[0059] The bulk density, fluidity and filling rate fluctuation of the comprehensive powder (maximum-minimum filling rate of five welding wires) are shown in Table 3.
[0060] Table 2 Content of chemical components of steel strips used in Examples 1-4
[0061] Chemical Elements C Mn Si S P N Ni Cr content(%) 0.012 1.35 0.033 0.001 0.0013 0.018 8.2 18.5
[0062] Table 3 Comprehensive powder bulk density, fluidity and offline filling rate fluctuation
[0063]
[0064]
[0065] Through the fine drawing process, the welding wire is drawn to the required specifications. Straighteners are installed in the fine drawing process and the layer winding process respectively to ensure that the produced welding wire has good linearity. The finished welding wire has a warp distance of ≤5mm and a rebound diameter of ≥1000mm.
[0066] The chemical composition of the welds of Examples 1-4 was tested respectively, and the chemical composition of the welds was shown in Table 3.
[0067] Table 3 Chemical composition content in Examples 1-4
[0068] C Mn Si S P Cr Ni Mo N Example 1 0.023 1.27 0.60 0.004 0.012 22.7 7.5 0.02 0.10 Example 2 0.025 1.21 0.61 0.004 0.013 23.3 8.2 0.05 0.13 Example 3 0.027 1.37 0.67 0.005 0.013 24.1 9.0 0.03 0.15 Example 4 0.024 1.33 0.70 0.005 0.014 25.1 9.8 0.04 0.17
[0069] The test plate was welded according to the relevant standard GB / T 17853-2018 and the process test was carried out. The process test results are shown in Table 4. The tensile test was carried out on the welded steel weld specimens, and the tensile strength is shown in Table 5.
[0070] Conventional flux-cored welding wire for duplex stainless steel, its model is TS2209-FC11, the diameter range includes 0.8 / 1.0 / 1.2 / 1.6mm, is a commonly used welding material, a carbon dioxide gas shielded welding wire, mainly used for welding stainless steel materials such as SUS2205.
[0071] Table 4 Process performance
[0072]
[0073] Table 5 Mechanical properties
[0074]
[0075] The basic principles and main features of the invention and the advantages of the invention are shown and described above.
[0076] The present invention is not limited by the above-mentioned embodiments. The above-mentioned embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall all fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. An economical flux-cored welding wire for duplex stainless steel, the flux-cored welding wire is composed of a steel strip outer skin and a flux core, and the raw material of the flux core is calculated by percentage to the total welding wire, including the following components: Alumina 0.05~0.15%; Metal chromium 1-1.5%; Nickel powder 0.15~0.4%; Zircon sand 0.08~0.24%; Bismuth oxide 0.01~0.03%; Cryolite 0.25~0.055%; Aluminum powder 0.025~0.045%; Rutile 0.9-1.2%; Quartz sand 0.025~0.4%; Ferrotitanium 0.04~0.12%; Electrolytic manganese 0.08~0.24%; Chromium ferronitride 0.15-0.24%; Potassium titanate 0.1~0.3%; Nanocrystalline high-purity spherical magnesium powder 0.04-0.12%; Teflon 0.01~0.03%, the balance is iron powder.
2. An economical flux-cored welding wire for duplex stainless steel as claimed in claim 1, characterized in that: The iron powder is reduced iron powder or atomized iron powder.
3. An economical flux-cored welding wire for duplex stainless steel as claimed in claim 1, characterized in that: Except for Teflon, the particle size range of each component of the drug core is -80 mesh to +160 mesh.
4. An economical flux-cored welding wire for duplex stainless steel as claimed in claim 1, characterized in that: The particle size of the Teflon is between -220 meshes and +375 meshes, and the friction coefficient is between 0.03 and 0.
15.
5. An economical flux-cored welding wire for duplex stainless steel as claimed in claim 1, characterized in that: The finished product specification of the flux-cored welding wire is 0.8mm-1.2mm.
6. An economical flux-cored welding wire for duplex stainless steel and a method for manufacturing the same, characterized in that: The following steps are involved: (1) Raw material processing process: The added rutile, quartz sand and zircon sand are calcined in a high temperature furnace at 900℃-1000℃ in trays, with the material placed on each tray not exceeding 50mm, and kept warm for 2h; The added alumina, cryolite and potassium titanate are calcined in a high temperature furnace at 450℃-550℃ in trays, with the material placed on each tray not exceeding 50mm, and kept warm for 2h; Prepare the raw material components of the core according to the proportion and bake at 220℃-270℃, keep warm for 2-3h, and stir the powder after it cools to no higher than 60℃ for 30-60min; (2) Powder filling process: After the steel strip is formed into a U-shaped groove by a roller, it is filled with 25%-27% powder, and the seam is overlapped during the seam joining process; (3) Fine drawing process and layer winding process: A calibrator is installed in the fine drawing process and layer winding process.
Citation Information
Cited By
Ultra-low carbon duplex stainless steel all-position welding flux-cored wire and welding method thereof
CN120269213A