Composite coal-based hard carbon as well as preparation method and application thereof

By preparing composite coal-based hard carbon materials, the problem of insufficient conductivity of the negative electrode material of sodium ion battery is solved, and the battery performance with high specific capacity and high efficiency is achieved, which is suitable for the negative electrode material of sodium ion battery.

CN119018877APending Publication Date: 2024-11-26GANZHOU LITAN NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411119143.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing negative electrode materials of sodium ion batteries cannot meet the commercial needs. The crystal layer spacing of traditional graphite materials and the hexagonal arrangement of carbon atoms are not suitable for the embedding of sodium ions, resulting in insufficient conductivity and it is difficult to improve the specific capacity of the battery and the first time. Coulomb efficiency.

Method used

Using composite coal-based hard carbon materials, the mixture and carbonization of pre-oxidized coal-based hard carbon with crosslinking agent and hard carbon precursor is formed to form composite coal-based hard carbon with high specific capacity and first Coulomb efficiency as the negative electrode of sodium ion battery. Material.

Benefits of technology

The high specific capacity (>280mAh/g) and high first-time Coulomb efficiency (>88%) of composite coal-based hard carbon were achieved, and the powder compaction density was improved, significantly improving the performance of sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018877A_ABST
    Figure CN119018877A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery negative electrode materials, and particularly relates to composite coal-based hard carbon as well as a preparation method and application thereof. According to the invention, partial oxygen-containing groups in the pre-oxidized coal-based raw material and the hard carbon precursor can be subjected to polar bond breakage and substitution under the action of free radical groups formed by decomposition of the cross-linking agent, so that cross-linking is realized. The composite coal-based hard carbon obtained through the carbonization process has better powder compaction density, high gram volume and first coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery negative electrode materials, and specifically relates to a composite coal-based hard carbon and a preparation method and application thereof. Background Art

[0002] The increasing depletion of traditional non-renewable energy and the environmental pollution caused by the use of fossil fuels have brought great challenges to the development of human society in the 21st century, and the demand for the development of renewable energy has become increasingly urgent. However, the existing secondary energy has the characteristics of unstable power generation and cannot be directly incorporated into the existing power grid, but the existing power grid has the need to reduce peaks and fill valleys. In the process of meeting the above needs, the existence of secondary electron energy storage can make up for part of the energy gap.

[0003] Sodium-ion batteries have become the most promising alternative to lithium-ion batteries in large-scale grid energy storage in recent years because of their high sodium abundance, low cost, and similar energy storage mechanism to lithium-ion batteries. At present, the main constraint on the development of sodium-ion batteries is the negative electrode material. Because the crystal interlayer spacing of graphite materials and the hexagonal arrangement of carbon atoms are not suitable for the embedding of sodium ions, traditional graphite materials cannot be used in the field of sodium-ion batteries. Soft carbon materials have fewer defects, smaller carbon interlayer spacing, and much better conductivity than hard carbon materials. From the research experience of negative electrode materials for lithium-ion batteries, it can be seen that conductivity is a key factor affecting the rate performance of negative electrode materials. By compounding soft carbon and hard carbon, and taking advantage of the good conductivity of soft carbon and the rich sodium storage active sites of hard carbon, it is expected to prepare negative electrode materials with excellent performance. Amorphous carbon materials made from coal with a high carbon content, especially hard carbon materials, are likely to be used as the core materials for the negative electrode of sodium-ion batteries. Coal-based carbon materials represented by sub-bituminous coal, bituminous coal, and anthracite are abundant in resources and low in price. Developing carbon materials with coal-based carbon as the main raw material and applying them to lithium-ion batteries and sodium-ion batteries is not only beneficial to saving energy, reducing pollution, improving battery power characteristics and low-temperature applicability, but also can effectively reduce battery costs.

[0004] A Chinese patent with publication number CN111293309A discloses a method for improving the performance of coal-based sodium-ion battery negative electrode materials and its application. The patent mixes coal-based materials with soft carbon precursors, treats them at low temperature in an air atmosphere, and then carbonizes them at high temperature to obtain an amorphous carbon material with a sodium storage capacity of about 220mAh / g and an initial coulombic efficiency of 80%. The amorphous carbon material uses coal-based materials as raw materials, but its capacity and efficiency are difficult to meet the requirements of commercial sodium-ion batteries. Although the carbon material of this invention has a significant improvement in specific capacity, the initial coulombic efficiency of only 80% makes it difficult to actually apply it commercially. Summary of the invention

[0005] The object of the present invention is to provide a composite coal-based hard carbon and a preparation method and application thereof. The composite coal-based hard carbon provided by the present invention can have both high specific capacity and first coulombic efficiency.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing composite coal-based hard carbon, comprising the following steps:

[0008] Pre-oxidizing the coal raw material to obtain pre-oxidized coal material;

[0009] The pre-oxidized coal material, the cross-linking agent and the hard carbon precursor are mixed to obtain a composite coal-based hard carbon precursor;

[0010] Under a protective atmosphere, sequentially subjecting the composite coal-based hard carbon precursor to a first carbonization and a second carbonization to obtain the composite coal-based hard carbon;

[0011] The temperature of the first carbonization is lower than the temperature of the second carbonization;

[0012] The hard carbon precursor includes one or more of phenolic resin, epoxy resin, polypropylene chloride resin and polyethylene composite material.

[0013] Preferably, the coal raw material includes one or more of bituminous coal, anthracite and sub-bituminous coal.

[0014] Preferably, the pre-oxidation temperature is 300-500° C. and the time is 2-6 hours.

[0015] Preferably, the crosslinking agent includes one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, di-tert-butyl peroxide, p-benzoylquinone dioxime, p-benzoquinone dioxime and bismaleimide.

[0016] Preferably, the mass ratio of the pre-oxidized coal material, the cross-linking agent and the hard carbon precursor is 1:0.003-0.01:0.02-1.

[0017] Preferably, the mass ratio of the pre-oxidized coal material, the cross-linking agent and the hard carbon precursor is 1:0.006:0.5.

[0018] Preferably, the temperature of the first carbonization is 500-700° C., and the holding time is 1-4 hours; the temperature of the second carbonization is 1000-1400° C., and the holding time is 2-6 hours.

[0019] Preferably, the protective atmosphere includes one or more of nitrogen, helium, neon, argon, krypton and xenon.

[0020] The present invention also provides a composite coal-based hard carbon prepared by the preparation method described in the above technical solution, wherein the particle size of the composite coal-based hard carbon is D50: 5 to 12 μm.

[0021] The present invention also provides the use of the composite coal-based hard carbon described in the above technical solution as a negative electrode material in a battery.

[0022] The present invention provides a method for preparing composite coal-based hard carbon, comprising the following steps: pre-oxidizing coal raw materials to obtain pre-oxidized coal; mixing the pre-oxidized coal, a cross-linking agent and a hard carbon precursor to obtain a composite coal-based hard carbon precursor; subjecting the composite coal-based hard carbon precursor to a first carbonization and a second carbonization in sequence under a protective atmosphere to obtain the composite coal-based hard carbon; the temperature of the first carbonization is lower than the temperature of the second carbonization; the hard carbon precursor comprises one or more of phenolic resin, epoxy resin, polypropylene chloride resin and polyethylene composite material. In the present invention, part of the oxygen-containing groups in the pre-oxidized coal-based raw materials can undergo polar bond breaking and substitution with the hard carbon precursor under the action of free radicals formed after the decomposition of the cross-linking agent to achieve cross-linking. The composite coal-based hard carbon obtained through the carbonization process has better powder compaction density, high gram capacity and first coulomb efficiency.

[0023] The present invention also provides a composite coal-based hard carbon prepared by the preparation method described in the above technical solution, wherein the particle size of the composite coal-based hard carbon is D50: 5-12 μm. The specific capacity of the composite coal-based hard carbon is greater than 280 mAh / g, the first coulomb efficiency is greater than 88%, and the powder compaction is greater than 1.1 g / cm 3 , and its performance is better than that of pure coal-based hard carbon negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of the composite coal-based hard carbon prepared in Example 2;

[0025] Figure 2 This is a charge and discharge curve diagram of the composite coal-based hard carbon prepared in Example 2 used as a negative electrode material in a sodium ion battery. DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing composite coal-based hard carbon, comprising the following steps:

[0027] Pre-oxidizing the coal raw material to obtain pre-oxidized coal material;

[0028] The pre-oxidized coal material, the cross-linking agent and the hard carbon precursor are mixed to obtain a composite coal-based hard carbon precursor;

[0029] Under a protective atmosphere, sequentially subjecting the composite coal-based hard carbon precursor to a first carbonization and a second carbonization to obtain the composite coal-based hard carbon;

[0030] The temperature of the first carbonization is lower than the temperature of the second carbonization;

[0031] The hard carbon precursor includes one or more of phenolic resin, epoxy resin, polypropylene chloride resin and polyethylene composite material.

[0032] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0033] The present invention pre-oxidizes the coal raw material to obtain the pre-oxidized coal material.

[0034] In the present invention, the coal raw material preferably includes one or more of bituminous coal, anthracite and sub-bituminous coal, and more preferably bituminous coal.

[0035] In the present invention, when the coal raw material is bituminous coal, bituminous coal has a lower degree of coalification than anthracite, contains more unstable aromatic hydrocarbon side chains, and has a deeper degree of pre-oxidation. The pre-oxidized coal material formed has more oxygen-containing functional groups, and the degree of cross-linking reaction after blending with a cross-linking agent and a hard carbon precursor is deeper.

[0036] In the present invention, the pre-oxidation is preferably carried out in an air atmosphere, and the air atmosphere is preferably a static air atmosphere; the pre-oxidation temperature is preferably 300-500°C, and more preferably 300°C; the pre-oxidation time is preferably 2-6h, and more preferably 3h.

[0037] After the pre-oxidation is completed, the present invention also preferably includes naturally cooling the obtained coal material to room temperature and crushing it in sequence. In the present invention, the crushing process preferably includes mechanical crushing and air flow pulverization in sequence; the particle size D50 of the material after the mechanical crushing is preferably 0.1 to 28 mm; the particle size D50 of the material after the air flow pulverization is preferably 1 to 50 μm.

[0038] After obtaining the preoxidized coal material, the present invention mixes the preoxidized coal material, a crosslinking agent and a hard carbon precursor to obtain a composite coal-based hard carbon precursor.

[0039] In the present invention, the cross-linking agent preferably includes one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, di-tert-butyl peroxide, p-benzoylquinone dioxime, p-benzoquinone dioxime and bismaleimide, and is further preferably 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.

[0040] In the present invention, when the cross-linking agent is di-tert-butyl peroxide, the OO bond in the cross-linking agent can undergo homolytic cleavage to generate free radicals to initiate a coupling reaction between the pre-oxidized coal and the hard carbon precursor, and cross-linking occurs to form a cross-linked network structure, which enhances the rigidity of the structure to a certain extent, improves the compaction density of the carbonized product, and obtains a sodium negative electrode material with high coulombic efficiency, large specific capacity and high compaction density for the first time.

[0041] In the present invention, the hard carbon precursor includes one or more of phenolic resin, epoxy resin, polypropylene chloride resin and polyethylene composite material, and is more preferably polypropylene chloride resin.

[0042] In the present invention, the cross-linking agent is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane. When the hard carbon precursor is polypropylene chloride resin, the cross-linking agent can undergo a dehalogenation reaction with the chlorine on the polypropylene chloride resin, and cross-linking occurs to form a cross-linked network structure. The introduction of the cross-linked structure greatly enhances the disorder of the carbonized product, expands its interlayer spacing and the number of closed pores, and the polypropylene chloride resin can increase the density of coal, improve the weight and quality of coal, and to a certain extent, can improve the compaction density of the carbonized product.

[0043] In the present invention, the mass ratio of the pre-oxidized coal material, the cross-linking agent and the hard carbon precursor is preferably 1:0.003-0.01:0.02-1, more preferably 1:0.006-0.01:0.02-1, and more preferably 1:0.006:0.5.

[0044] After obtaining the composite coal-based hard carbon precursor, the present invention sequentially performs a first carbonization and a second carbonization on the composite coal-based hard carbon precursor under a protective atmosphere to obtain the composite coal-based hard carbon;

[0045] The temperature of the first carbonization is lower than the temperature of the second carbonization.

[0046] In the present invention, the protective atmosphere preferably includes one or more of nitrogen, helium, neon, argon, krypton and xenon, and more preferably argon.

[0047] In the present invention, the temperature of the first carbonization is preferably 500-700°C, more preferably 700°C; the time of the first carbonization is preferably 1-4h, more preferably 2h; the first carbonization is preferably carried out in an atmosphere rotary kiln. In the present invention, the flow rate of the protective atmosphere is preferably 0.5-2L / min. In the present invention, since the atmosphere rotary kiln has a certain stirring effect, setting a certain rotation speed during the first carbonization process can make the pre-oxidized coal material fully cross-linked and cured with the cross-linking agent and the hard carbon precursor.

[0048] After the first carbonization is completed, the present invention also preferably includes mechanically breaking up and sieving the composite coal-based hard carbon precursor after the first carbonization; the particle size of the material after the sieving treatment is preferably 9 to 10 μm. In the present invention, after the first carbonization, part of the cross-linking agent is cross-linked with the coal material and the hard carbon precursor, and agglomeration may occur after solidification, so the presence of mechanical breaking up and sieving treatment can control the particle size to the required range through the breaking up equipment.

[0049] In the present invention, the temperature of the second carbonization is preferably 1000-1400°C, more preferably 1200°C; the time of the second carbonization is preferably 2-6h, more preferably 4h; the heating rate of the second carbonization is preferably 3-5°C / min; the second carbonization is preferably carried out in a box-type atmosphere furnace. In the present invention, the flow rate of the protective atmosphere is preferably 5-15L / min. In the present invention, the second carbonization can cause the composite coal-based hard carbon precursor after the first carbonization to undergo a cracking reaction.

[0050] After the second carbonization is completed, the present invention also preferably includes naturally cooling the product after the second carbonization to room temperature in a furnace to obtain the composite coal-based hard carbon.

[0051] The present invention also provides a composite coal-based hard carbon prepared by the preparation method described in the above technical solution, wherein the particle size of the composite coal-based hard carbon is D50: 5-12 μm. In the present invention, the specific capacity of the composite coal-based hard carbon is preferably greater than 280 mAh / g, the first coulomb efficiency is preferably greater than 88%, and the powder compaction is preferably ≥1.1 g / cm 3 , and its performance is better than that of pure coal-based hard carbon negative electrode materials.

[0052] In order to further illustrate the present invention, a composite coal-based hard carbon and its preparation method and application provided by the present invention are described in detail below in combination with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.

[0053] Example 1

[0054] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal is pre-oxidized using air in the environment at a temperature of 300°C for 3 hours. The pre-oxidized coal is obtained after natural cooling.

[0055] The preoxidized coal material is mechanically crushed and air flow milled to obtain a preoxidized coal powder material with a particle size of D50: 8.7 μm. The preoxidized coal powder material, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and polypropylene chloride resin are mechanically uniformly mixed in a mass ratio of 1:0.006:0.02 to obtain a composite coal-based hard carbon precursor.

[0056] The composite coal-based hard carbon precursor was transferred to an atmosphere rotary kiln and subjected to the first carbonization under a nitrogen atmosphere at a temperature of 700°C for 2 hours. The composite coal-based hard carbon precursor that had completed the first carbonization was crushed and sieved, and the particle size of the sieved material was D50: 9.0 μm. It was then transferred to a box furnace for the second carbonization, with a heating rate of 5°C / min, a temperature of 1200°C, and a holding time of 4 hours. After cooling in the furnace, the composite coal-based hard carbon was obtained.

[0057] Example 2

[0058] The other preparation processes and conditions in Example 1 remain unchanged, except that the pre-oxidized coal, the cross-linking agent and the hard carbon precursor are mixed in a mass ratio of 1:0.006:0.5 to prepare a composite coal-based hard carbon.

[0059] Example 3

[0060] The other preparation processes and conditions in Example 1 remain unchanged, except that the pre-oxidized coal material, the cross-linking agent and the hard carbon precursor are mixed in a mass ratio of 1:0.006:1 to prepare a composite coal-based hard carbon.

[0061] Example 4

[0062] The other preparation processes and conditions in Example 1 remain unchanged, except that the pre-oxidized coal material, the cross-linking agent and the hard carbon precursor are mixed in a mass ratio of 1:0.01:0.5 to prepare a composite coal-based hard carbon.

[0063] Example 5

[0064] The other preparation processes and conditions in Example 1 remain unchanged, except that the pre-oxidized coal, the cross-linking agent and the hard carbon precursor are mixed in a mass ratio of 1:0.003:0.5 to prepare a composite coal-based hard carbon.

[0065] Example 6

[0066] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal is pre-oxidized using air in the environment at a temperature of 300°C for 3 hours. The pre-oxidized coal is obtained after natural cooling.

[0067] The preoxidized coal material is mechanically crushed and air flow milled to obtain a preoxidized coal powder material with a particle size of D50: 9.2 μm. The preoxidized coal powder material, benzoyl peroxide and epoxy resin are mechanically and uniformly mixed in a mass ratio of 1:0.006:0.5 to obtain a composite coal-based hard carbon precursor.

[0068] The composite coal-based hard carbon precursor was transferred to an atmosphere rotary kiln and subjected to the first carbonization under an argon atmosphere at a temperature of 700°C for 2 hours. The composite coal-based hard carbon precursor that had completed the first carbonization was crushed and sieved, and the particle size of the sieved material was D50: 9.4μm. It was then transferred to a box furnace for the second carbonization at a temperature of 1200°C, a heating rate of 5°C / min, and a holding time of 4 hours. After cooling in the furnace, the composite coal-based hard carbon was obtained.

[0069] In the present embodiment, during the low-temperature firing process, the active hydroxyl groups contained in the oxidized coal material undergo a hydroxycarbonyl condensation reaction with the carbonyl groups on the epoxy resin under the action of the crosslinking agent benzoyl peroxide, and crosslinking occurs to form a crosslinked network structure.

[0070] Example 7

[0071] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal is pre-oxidized using air in the environment at a temperature of 300°C for 3 hours. The pre-oxidized coal is obtained after natural cooling.

[0072] The preoxidized coal material is mechanically crushed and air flow milled to obtain a preoxidized coal powder material with a particle size of D50: 9.2 μm. The preoxidized coal powder material, p-benzoylquinone dioxime and epoxy resin are mechanically and uniformly mixed in a mass ratio of 1:0.006:0.5 to obtain a composite coal-based hard carbon precursor.

[0073] The composite coal-based hard carbon precursor was transferred to an atmosphere rotary kiln and subjected to the first carbonization under a nitrogen atmosphere at a temperature of 700°C for 2 hours. The composite coal-based hard carbon precursor that had completed the first carbonization was crushed and sieved, and the particle size of the sieved material was D50: 9.4μm. It was then transferred to a box furnace for the second carbonization at a temperature of 1200°C for 4 hours, and the composite coal-based hard carbon was obtained after cooling in the furnace.

[0074] Example 8

[0075] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal is pre-oxidized using air in the environment at a temperature of 300°C for 3 hours. The pre-oxidized coal is obtained after natural cooling.

[0076] The preoxidized coal material is mechanically crushed and air flow milled to obtain a preoxidized coal powder material with a particle size of D50: 9.2 μm. The preoxidized coal powder material, p-benzoquinone dioxime and polypropylene chloride resin are mechanically and uniformly mixed in a mass ratio of 1:0.006:0.5 to obtain a composite coal-based hard carbon precursor.

[0077] The composite coal-based hard carbon precursor was transferred to an atmosphere rotary kiln and subjected to the first carbonization under a nitrogen atmosphere at a temperature of 700°C for 2 hours. The composite coal-based hard carbon precursor that had completed the first carbonization was crushed and sieved, and the particle size of the sieved material was D50: 9.4μm. It was then transferred to a box furnace for the second carbonization at a temperature of 1200°C for 4 hours, and the composite coal-based hard carbon was obtained after cooling in the furnace.

[0078] Example 9

[0079] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal is pre-oxidized using air in the environment at a temperature of 300°C for 3 hours. The pre-oxidized coal is obtained after natural cooling.

[0080] The preoxidized coal material is mechanically crushed and air flow milled to obtain a preoxidized coal powder material with a particle size of D50: 9.2 μm. The preoxidized coal powder material, bismaleimide and epoxy resin are mechanically and uniformly mixed in a mass ratio of 1:0.006:0.5 to obtain a composite coal-based hard carbon precursor.

[0081] The composite coal-based hard carbon precursor was transferred to an atmosphere rotary kiln and subjected to the first carbonization under a nitrogen atmosphere at a temperature of 700°C for 2 hours. The composite coal-based hard carbon precursor that had completed the first carbonization was crushed and sieved, and the particle size of the sieved material was D50: 9.4μm. It was then transferred to a box furnace for the second carbonization at a temperature of 1200°C for 4 hours, and the composite coal-based hard carbon was obtained after cooling in the furnace.

[0082] Example 10

[0083] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal is pre-oxidized using air in the environment at a temperature of 300°C for 3 hours. The pre-oxidized coal is obtained after natural cooling.

[0084] The preoxidized coal material is mechanically crushed and air flow milled to obtain a preoxidized coal powder material with a particle size of D50: 9.2 μm. The preoxidized coal powder material, di-tert-butyl peroxide and polypropylene chloride resin are mechanically and uniformly mixed in a mass ratio of 1:0.006:0.5 to obtain a composite coal-based hard carbon precursor.

[0085] The composite coal-based hard carbon precursor was transferred to an atmosphere rotary kiln for the first carbonization under a nitrogen atmosphere at a temperature of 700°C for 2 hours. The composite coal-based hard carbon precursor that had completed the first carbonization was crushed and sieved, and the particle size of the sieved material was D50: 9.4μm. It was then transferred to a box furnace for the second carbonization at a temperature of 1200°C for 4 hours, and the composite coal-based hard carbon was obtained after cooling with the furnace.

[0086] Comparative Example 1

[0087] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal material is oxidized by using the air in the environment. The oxidation temperature is 300°C and the treatment time is 3h. After natural cooling, the pre-oxidized coal material is obtained.

[0088] The pre-oxidized coal material was mechanically crushed and air flow milled to obtain a powder material with a particle size of D50: 9.0 μm. The pre-oxidized coal powder material was mechanically mixed with 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane at a mass ratio of 1:0.006, and then transferred to a rotary kiln for low-temperature roasting at 700°C for 2 hours under a nitrogen atmosphere, and then calcined in a box furnace at 1200°C for 4 hours and then cooled with the furnace to obtain a composite coal-based hard carbon.

[0089] Comparative Example 2

[0090] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal material is oxidized by using the air in the environment. The oxidation temperature is 300°C and the treatment time is 3h. After natural cooling, the pre-oxidized coal material is obtained.

[0091] The pre-oxidized coal was mechanically crushed and air flow milled to obtain powder with a particle size of D50: 9.3 μm. The pre-oxidized coal was mechanically mixed with polypropylene chloride resin at a mass ratio of 1:0.5, and then transferred to a rotary kiln for low-temperature roasting at 700°C for 2 hours in a nitrogen atmosphere, and then heated to 1200°C in a box furnace for 4 hours and then cooled with the furnace to obtain composite coal-based hard carbon.

[0092] Comparative Example 3

[0093] The bituminous coal raw material is put into an atmosphere rotary furnace for open firing, and the coal material is oxidized by using the air in the environment. The oxidation temperature is 300°C and the treatment time is 3h. After natural cooling, the pre-oxidized coal material is obtained.

[0094] The pre-oxidized coal was mechanically crushed and air flow milled to obtain powder with a particle size of D50: 8.9 μm. The pre-oxidized coal was transferred to a rotary kiln for low-temperature roasting at 700°C for 2 hours under a nitrogen atmosphere, and then calcined at 1200°C in a box furnace for 4 hours and then cooled with the furnace to obtain composite coal-based hard carbon.

[0095] Performance Testing

[0096] (1) True density test: The composite coal-based hard carbon samples prepared in Examples 1 to 10 and Comparative Examples 1 to 3 are placed in a true density tester. Helium is used as the medium. The measuring chamber is gradually pressurized to a specified value. The helium is then expanded into the expansion chamber. The equilibrium pressure of the two processes is automatically recorded by the instrument. According to the law of conservation of mass, the volume of the measuring chamber and the expansion chamber is calibrated by a standard ball, and then the volume of the sample is determined to calculate the true density.

[0097] Table 1 True density and powder compaction density of composite coal-based hard carbon prepared in Examples and Comparative Examples

[0098]

[0099] (2) The composite coal-based hard carbons prepared in Examples 1 to 10 and Comparative Examples 1 to 3 were used as active materials for negative electrode materials of sodium ion batteries to prepare button batteries. The preparation process was as follows:

[0100] In a drying room with a humidity of less than 10%, composite coal-based hard carbon, conductive carbon black and binder are mixed in NMP at a mass ratio of 90:5:5, homogenized, and the solid content is controlled at 45%. The mixture is coated on an aluminum foil current collector, vacuum-baked at 100-110° C. for 4-8 hours, pressed into shape, and then punched into a negative electrode sheet for a sodium ion battery.

[0101] A button half-cell was assembled in a glove box filled with argon. The counter electrode was a metal sodium sheet, the separator used was PE, and the electrolyte was 1 mol / L NaPF6 (EC / DMCVol1:1). The button cell was subjected to charge and discharge tests. The test process was 0.1C discharge to 0V, 0V constant voltage to 0.03C, and 0.1C charge to 2V. The first reversible capacity and efficiency of the sodium negative electrode material in the embodiment and the comparative example were measured. The button cell test equipment was the commercial LAND battery test system of Wuhan Landian Electronics Co., Ltd.

[0102] The button-type batteries prepared by using the composite coal-based hard carbon prepared in Examples 1 to 10 and Comparative Examples 1 to 3 as the active material of the negative electrode material of the sodium ion battery were subjected to electrochemical charge and discharge tests at a voltage range of 0V to 2V. The test results are shown in Table 2:

[0103] Table 2 Reversible capacity of composite hard carbon materials at charge and discharge current density in the examples and comparative examples

[0104]

[0105] Combining Table 1 and Table 2, we can see that:

[0106] Examples 1 to 3 and Comparative Example 1 adjusted the amount of hard carbon precursor added. The greater the amount of hard carbon precursor added, the compaction density of the finished product showed a trend of first increasing and then decreasing. When the addition ratio of the hard carbon precursor was 0.5, the compaction density, specific capacity, and first efficiency improvement effects were the most balanced. When the addition ratio was further increased to 1, the advantage of high compaction of composite coal-based hard carbon was balanced by the hard carbon precursor, thus showing a trend of decreasing compaction level, but its reversible specific capacity and first-efficiency coulomb efficiency were significantly improved, which was mainly due to the high reversible specific capacity and first coulomb efficiency shown by the hard carbon precursor after carbonization.

[0107] The improvement in the compaction density level of Comparative Example 1 compared to Comparative Example 3 can be explained as being mainly due to the effect of the cross-linking agent, while the improvement in specific capacity is not obvious.

[0108] Compared with the specific capacity improvement effect of Comparative Example 2 compared with that of Comparative Example 3, the hard carbon precursor has a more obvious effect in improving the specific capacity.

[0109] The amount of cross-linking agent added was adjusted in Example 2, Example 4, Example 5, and Comparative Example 2. When the cross-linking agent addition ratio was 0.006, the compacted density, reversible specific capacity, and first coulombic efficiency were significantly improved. When the cross-linking agent addition ratio was increased to 0.003, the compacted density improvement effect was weaker than when the addition ratio was 0.006, but as the cross-linking agent addition ratio increased to 0.01, the compacted density improvement effect was weaker than when the addition ratio was 0.006, and there was an inhibitory effect on the improvement of the reversible specific capacity and the first coulombic efficiency, so the cross-linking agent ratio was preferably 0.006.

[0110] Examples 6 to 10 changed the type of crosslinking agent and the type of hard carbon precursor compared to Example 2. In Example 6, during the low-temperature firing process, the active hydroxyl groups contained in the oxidized coal material reacted with the carbonyl groups on the epoxy resin under the action of the crosslinking agent benzoyl peroxide to form a crosslinked network structure.

[0111] The SEM image of the composite coal-based hard carbon prepared in Example 2 is as follows: Figure 1 The charge and discharge curve of the composite coal-based hard carbon prepared in Example 2 as a negative electrode material for sodium ion batteries is shown in FIG. Figure 2 shown.

[0112] In Example 2, when the hard carbon precursor is polypropylene chloride resin and the crosslinking agent is 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, the powder compaction density is higher and the performance balance point of the sodium gram capacity level and the first coulomb efficiency is optimal.

[0113] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing composite coal-based hard carbon, characterized in that: The following steps are involved: Pre-oxidizing the coal raw material to obtain pre-oxidized coal material; The pre-oxidized coal material, the cross-linking agent and the hard carbon precursor are mixed to obtain a composite coal-based hard carbon precursor; Under a protective atmosphere, sequentially subjecting the composite coal-based hard carbon precursor to a first carbonization and a second carbonization to obtain the composite coal-based hard carbon; The temperature of the first carbonization is lower than the temperature of the second carbonization; The hard carbon precursor includes one or more of phenolic resin, epoxy resin, polypropylene chloride resin and polyethylene composite material.

2. The preparation method according to claim 1, characterized in that: The coal raw material includes one or more of bituminous coal, anthracite and sub-bituminous coal.

3. The preparation method according to claim 1 or 2, characterized in that: The pre-oxidation temperature is 300-500° C. and the time is 2-6 hours.

4. The preparation method according to claim 1, characterized in that: The crosslinking agent includes one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, di-tert-butyl peroxide, p-benzoylquinone dioxime, p-benzoquinone dioxime and bismaleimide.

5. The preparation method according to claim 1, characterized in that: The pre-oxidized coal 、 The mass ratio of the cross-linking agent to the hard carbon precursor is 1:0.003~0.01:0.02~1.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the pre-oxidized coal material, the cross-linking agent and the hard carbon precursor is 1:0.006:0.

5.

7. The preparation method according to claim 1, characterized in that: The temperature of the first carbonization is 500-700° C., and the insulation time is 1-4 hours; the temperature of the second carbonization is 1000-1400° C., and the insulation time is 2-6 hours.

8. The preparation method according to claim 1, characterized in that: The protective atmosphere includes one or more of nitrogen, helium, neon, argon, krypton and xenon.

9. The composite coal-based hard carbon prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The particle size D50 of the composite coal-based hard carbon is 5 to 12 μm.

10. Use of the composite coal-based hard carbon according to claim 9 as a negative electrode material in a battery.

Citation Information

Patent Citations

  • Sodion secondary battery negative electrode material and preparing method and application thereof

    CN105185997A

  • Performance improvement method and application of sodium-ion battery carbon-based negative electrode material

    CN113526489A

  • Coal-based carbon negative electrode material, preparation method and application thereof, and battery containing coal-based carbon negative electrode material

    CN114335522A

  • Coal-based hard carbon as well as preparation method and application thereof

    CN118004996A

  • Sodium ion battery negative electrode material and preparation method thereof

    CN118270758A

Cited By

  • Low-dimensional coal-based hard carbon material with high sodium storage capacity and high initial coulombic efficiency and preparation method of low-dimensional coal-based hard carbon material

    CN119612493A

  • A low-dimensional coal-based hard carbon material with both high sodium storage capacity and high initial coulombic efficiency and its preparation method.

    CN119612493B

  • Method and device for preparing hard carbon negative electrode material based on lignite

    CN121452824A

  • A lignite-based hard carbon negative electrode material preparation method and device

    CN121452824B