Method for efficiently reducing U (VI) in water through low-frequency ultrasonic-driven piezoelectric catalysis

Through low-frequency ultrasonic driving piezoelectric catalytic method, the built-in piezoelectric field reduces U(VI) in water, solves the problems of high energy consumption and complex management of traditional electrochemical reduction methods, and achieves efficient and low-consumption U(VI) removal. Reduces environmental pollution and by-product production.

CN119018989AInactive Publication Date: 2024-11-26EAST CHINA UNIV OF TECH

Patent Information

Application Number
CN202411451313.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional electrochemical reduction method requires additional power supply to reduce U(VI) in water, which has high energy consumption, complex operation and management, and has few research on heavy metal reduction, especially the reduction of radioactive U(VI).

Method used

Low-frequency ultrasonic drive piezoelectric catalytic method is used to generate a built-in piezoelectric field under the action of external mechanical force through piezoelectric catalyst, instead of external DC electric field, and use piezoelectric electron-hole pair to perform U(VI) reduction reaction to generate insoluble U(IV). The method includes placing the piezoelectric catalyst and hole inhibitor in a U(VI) solution, generating a built-in piezoelectric field through ultrasonic activation, causing the electrons to undergo a reduction reaction with U(VI).

Benefits of technology

It reduces energy consumption and operating costs, simplifies the operation process, significantly improves the reduction efficiency of U(VI), reduces environmental pollution, and produces fewer by-products, improving the cleanliness and safety of the processing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018989A_ABST
    Figure CN119018989A_ABST
Patent Text Reader

Abstract

The invention relates to the field of environmental water treatment, in particular to a method for efficiently reducing U (VI) in water through low-frequency ultrasonic-driven piezoelectric catalysis, which comprises the following steps: placing a piezoelectric catalyst in a solution containing U (VI), stirring in a magnetic stirrer to reach adsorption equilibrium under a dark state condition, placing the U (VI) solution containing the piezoelectric catalyst in an ultrasonic container, and stirring in a magnetic stirrer to reach adsorption equilibrium under a dark state condition; ultrasonic is used as piezoelectric driving force, and soluble U (VI) is reduced into insoluble U (IV) through piezoelectric catalysis. The piezoelectric catalyst is spontaneously polarized under the action of ultrasonic waves to generate piezoelectric electron-hole pairs, and the piezoelectric electron-hole pairs are driven to be separated and migrated to the surface of the piezoelectric catalyst under the action of a built-in piezoelectric field to participate in a reduction reaction. The built-in micro electric field generated through piezoelectric catalysis is used for replacing a traditional external direct-current electric field to reduce U (VI), operation management is easy, energy consumption and operation cost are reduced, and the potential of efficiently reducing metal in water is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of environmental water treatment, and in particular to a method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis. Background Art

[0002] Uranium ore is a raw material for the development of the nuclear industry. With the development of nuclear energy technology, the demand for uranium ore is increasing. Low-concentration radioactive nuclides will be produced during the mining, processing and transportation of uranium ore. These radioactive nuclides will enter the water environment under the influence of natural factors, causing great harm to the ecological environment. Uranium dissolved in water is mainly in the form of uranyl ions (UO2 2+ ) exists in the form of radiation, which can easily migrate with the flow of groundwater, enter the human body mainly through the food chain, and accumulate in the human body. The radiation produced during its decay process can damage human tissues, induce gene mutations, and increase the incidence of diseases such as tumors and cancers.

[0003] U(VI) complexes are highly soluble and have great radiotoxicity and chemical toxicity. Reducing the easily mobile U(VI) in the solution to the sparingly soluble U(IV) is an ideal strategy for treating uranium pollution. The electrochemical reduction method has high selectivity and no secondary pollution, and can efficiently reduce U(VI) in water, but it requires an external power supply, has high energy consumption, and is complex to operate and manage. Piezoelectric catalysis does not require an external power supply, is simple to operate and manage, can efficiently convert external mechanical energy into electrical energy, and has the potential to use the remaining mechanical energy in the environment to treat pollutants in water with low consumption. As an emerging water treatment technology, its principle is that when piezoelectric materials are subjected to external mechanical stress (such as ultrasonic vibration), polarized charges (piezoelectric electron-hole pairs) are generated, generating a built-in piezoelectric field. Under the action of the built-in piezoelectric field, the piezoelectric electron-hole pairs separate and migrate to the surface of the piezoelectric catalyst, participate in the redox reaction, and produce active species. At present, the research on piezoelectric catalytic technology is mainly focused on the oxidative degradation of organic pollutants, and there is little research on heavy metal reduction, especially the research on radioactive U(VI) reduction is extremely scarce.

[0004] The invention innovatively proposes to use the built-in piezoelectric field generated by piezoelectric catalysis to replace the external DC electric field to reduce U(VI) in water, and optimize the reduction effect by controlling the piezoelectric catalytic reaction conditions. The invention can provide an effective method and idea for the efficient and low-cost treatment of U(VI) in water. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the traditional electrochemical reduction method for reducing U(VI) in water, which requires an external power supply, has high energy consumption and complex operation and management, and provides a method for effectively reducing U(VI) in water by using piezoelectric catalysis to generate a built-in piezoelectric field instead of an external DC electric field to generate piezoelectric electrons.

[0006] To achieve the above objectives, the present invention provides the following technical solutions:

[0007] A method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis comprises a piezoelectric catalyst, an external mechanical force, a hole inhibitor, and a reaction container. The piezoelectric catalyst and the hole inhibitor are placed in a U(VI) solution to be treated, and the piezoelectric catalyst is activated by an external mechanical force to generate a built-in piezoelectric field, so that electrons and holes formed by the piezoelectric catalyst move in a direction toward the surface of the material under the action of the built-in piezoelectric field, and the hole concentration is suppressed under the action of the hole inhibitor, while electrons with a higher concentration react with U(VI) to generate U(IV).

[0008] The present invention achieves the above object through the following technical solutions:

[0009] A method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis comprises the following steps:

[0010] The piezoelectric catalyst is placed in a solution containing U(VI), stirred in a magnetic stirrer, and adsorption equilibrium is achieved under dark conditions.

[0011] After reaching adsorption equilibrium, the U(VI) solution containing the piezoelectric catalyst is placed in an ultrasonic container, methanol is added, and ultrasound is used as the piezoelectric driving force to reduce U(VI) through piezoelectric catalysis.

[0012] In the above solution, the piezoelectric catalyst is barium titanate or molybdenum disulfide.

[0013] In the above scheme, the concentration of U(VI) is 2-15 mg / L.

[0014] In the above scheme, the amount of piezoelectric catalyst used is 0.5-2.5 g / L.

[0015] In the above scheme, the pH of the U(VI) solution is 2.9-11.

[0016] In the above scheme, the ultrasonic frequency is 40kHz and the ultrasonic power is 40-300W.

[0017] In the above scheme, the adsorption equilibrium time is 20 min and the ultrasonic reaction time is 20 min.

[0018] The piezoelectric catalyst can convert ultrasonic mechanical energy into electrical energy.

[0019] The piezoelectric catalyst is pretreated before use, including cleaning, drying and activation steps.

[0020] In the reduction reaction of the piezoelectric catalyst driven by ultrasound, methanol is added as a hole inhibitor to adjust the separation efficiency of the piezoelectric electron-hole pairs.

[0021] After completing a reduction reaction, the piezoelectric catalyst is regenerated by a physical or chemical method to restore its activity for subsequent multiple cycles of use.

[0022] Compared with traditional electrochemical reduction technology, the beneficial effects of the present invention are: 1. The present invention utilizes the spontaneous polarization of piezoelectric catalysts under the action of external mechanical force (ultrasound) to generate polarized charges (piezoelectric electron-hole pairs). Under the action of the built-in piezoelectric field, the piezoelectric electron-hole pairs separate and migrate to the surface of the piezoelectric catalyst to participate in the reduction reaction. Its energy conversion mechanism can avoid the traditional electrochemical reduction method's dependence on external power sources, thereby reducing energy consumption and operating costs.

[0023] 2. The method used in the present invention is easy to operate. Compared with traditional electrochemical reduction which requires complex circuits and power management, piezoelectric catalysis is simpler and the catalytic process can be started by simply controlling the ultrasonic frequency and power, which greatly simplifies the equipment requirements and operating procedures.

[0024] 3. The present invention can significantly improve the reduction efficiency of U(VI) in water by optimizing the piezoelectric catalytic reaction conditions, including the type of piezoelectric catalyst, the dosage of piezoelectric catalyst, the pH value of the solution, and the ultrasonic power, thereby facilitating the effective removal of U(VI) in water and reducing environmental pollution.

[0025] 4. The present invention uses a catalyst with good stability and the reaction conditions are relatively mild. Compared with the problem of many by-products caused by the high redox potential of the traditional electrochemical reduction method, the piezoelectric catalytic reduction U(VI) process used in the present invention produces fewer harmful by-products, and the generation of the built-in piezoelectric field does not require the addition of additional chemicals, further improving the cleanliness and safety of the treatment process.

[0026] 5. The method of the present invention has wide applicability and high selectivity of the piezoelectric catalyst. It can not only effectively reduce U(VI), but is also applicable to other heavy metal ions with similar properties, and has good adaptability and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The reduction effects of the ultrasonic-molybdenum disulfide piezoelectric catalytic system, molybdenum disulfide catalytic system, and ultrasonic system on U(VI) in Example 1, Comparative Example 1, and Comparative Example 2 are shown;

[0028] Figure 2 The reduction effects of the ultrasonic-barium titanate piezoelectric catalytic system, the barium titanate catalytic system, and the ultrasonic system on U(VI) in Example 1, Comparative Example 1, and Comparative Example 2 are shown;

[0029] Figure 3 The piezoelectric catalytic reduction effect of U(VI) at different initial U(VI) concentrations in Example 2;

[0030] Figure 4 The reduction effect of U(VI) in water at different dosages of molybdenum disulfide piezoelectric catalysts in Example 3;

[0031] Figure 5 The reduction effect of U(VI) in water at different initial pH values ​​in Example 4;

[0032] Figure 6 This is the reduction effect of U(VI) in water under different ultrasonic powers in Example 5. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with specific embodiments.

[0034] In the following examples, the U(VI) reduction efficiency was calculated according to the following formula:

[0035] R=(C 0 -C) / C 0 *100%

[0036] R: Reduction efficiency

[0037] C 0 :U(VI) initial concentration

[0038] C: U(VI) concentration after reduction reaction.

[0039] The following examples use deionized water and ethanol to clean the piezoelectric catalyst to remove surface impurities, use vacuum drying or oven drying at 100°C for 5 hours to ensure complete drying, and use heat treatment activation. The piezoelectric catalyst is placed in a muffle furnace and activated at 500°C for 3 hours under a nitrogen atmosphere;

[0040] Using methanol as a vacancy inhibitor, add 2 mL of methanol to 100 mL of U(VI) solution;

[0041] Select acid washing regeneration, use 1mol / L dilute hydrochloric acid or 0.5mol / L dilute nitric acid to soak the catalyst for 3 hours, then rinse it with deionized water until it is neutral, and then activate it after drying.

[0042] Example 1: Weigh 2 portions of 100 mL of a 5 mg / L U(VI) solution, adjust the solution pH to 2.9 using dilute hydrochloric acid or sodium hydroxide, add 100 mg of molybdenum disulfide and barium titanate, respectively, and stir the reaction system in the dark for 20 min to reach adsorption-desorption equilibrium before reacting;

[0043] The ultrasonic generator was turned on for reaction, the ultrasonic frequency was 40kHz, the ultrasonic power was 300W, U(VI) was reduced by piezoelectric catalysis, the ultrasonic reaction time was 20min, samples were taken at regular intervals, filtered with a 0.22μm filter head, and the concentration of U(VI) in the solution was determined at 652nm using an ultraviolet spectrophotometer, and the color developer was arsenazo III;

[0044] The reduction effect of U(VI) after ultrasonic time using MoS2 piezoelectric catalyst is as follows Figure 1 As shown, the reduction efficiency is calculated to be 87.5% by substituting into the formula;

[0045] The reduction effect of U(VI) after ultrasonic time under the condition of barium titanate piezoelectric catalyst is shown in Figure 2. Figure 2 As shown, the reduction efficiency is calculated to be 62.8% by substituting into the formula.

[0046] Comparative Example 1: Weigh 2 portions of 100 mL of 5 mg / L U(VI) solution, adjust the solution pH to 2.9 with dilute hydrochloric acid or sodium hydroxide, add 100 mg of molybdenum disulfide and barium titanate, respectively, and stir the reaction system in the dark for 20 min to reach adsorption-desorption equilibrium before the reaction;

[0047] The reaction was carried out under indoor light for 20 minutes, and samples were taken at regular intervals, filtered using a 0.22 μm filter, and the concentration of U(VI) in the solution was determined at 652 nm using an ultraviolet spectrophotometer, with a chromogenic agent of arsenazo III.

[0048] The reduction effect of U(VI) after reaction using molybdenum disulfide piezoelectric catalyst is as follows Figure 1 As shown, the reduction efficiency is calculated to be 15.9% by substituting into the formula;

[0049] The reduction effect of U(VI) after reaction using barium titanate piezoelectric catalyst is as follows Figure 2 As shown, the reduction efficiency is calculated to be 19.6% by substituting it into the formula.

[0050] Comparative Example 2: Weigh 100 mL of a 5 mg / L U(VI) solution, adjust the pH of the solution to 2.9 using dilute hydrochloric acid or sodium hydroxide, and stir the reaction system in a dark place for 20 min before reacting;

[0051] The ultrasonic generator was turned on for reaction, the ultrasonic frequency was 40kHz, the ultrasonic power was 300W, U(VI) was reduced by piezoelectric catalysis, the ultrasonic reaction time was 20min, samples were taken at regular intervals, filtered with a 0.22μm filter head, and the concentration of U(VI) in the solution was determined at 652nm using an ultraviolet spectrophotometer, and the color developer was arsenazo III;

[0052] The reduction effect of U(VI) after ultrasonic time without piezoelectric catalyst is as follows Figure 1 and Figure 2 As shown, the reduction efficiency is calculated to be 0.08% by substituting it into the formula.

[0053] Example 2: Weigh 5 portions of 200 mL of U(VI) solution with concentrations of 2 mg / L, 5 mg / L, 8 mg / L, 10 mg / L, and 15 mg / L, respectively, adjust the pH of the solution to 2.9 using dilute hydrochloric acid or sodium hydroxide, add 200 mg of molybdenum disulfide, and stir the reaction system in the dark for 20 min to reach adsorption-desorption equilibrium before reacting;

[0054] The ultrasonic generator was turned on for reaction, the ultrasonic frequency was 40kHz, the ultrasonic power was 300W, U(VI) was reduced by piezoelectric catalysis, the ultrasonic reaction time was 20min, samples were taken at regular intervals, filtered with a 0.22μm filter head, and the concentration of U(VI) in the solution was determined at 652nm using an ultraviolet spectrophotometer, and the color developer was arsenazo III;

[0055] The reduction effect of MoS2 on U(VI) after ultrasonic treatment at different initial concentrations of U(VI) Figure 3 As shown, the reduction efficiencies calculated by substituting into the formula are 100%, 85.8%, 78.9%, 65.3% and 50.7%, respectively.

[0056] Example 3: Weigh 5 portions of 100 mL of a 5 mg / L U(VI) solution, adjust the pH of the solution to 2.9 using dilute hydrochloric acid or sodium hydroxide, add 100 mg, 200 mg, 300 mg, 400 mg, and 500 mg of molybdenum disulfide, respectively, and stir the reaction system in a dark place for 20 min to reach adsorption-desorption equilibrium before reacting;

[0057] The ultrasonic generator was turned on for reaction, the ultrasonic frequency was 40kHz, the ultrasonic power was 300W, U(VI) was reduced by piezoelectric catalysis, the ultrasonic reaction time was 20min, samples were taken at regular intervals, filtered with a 0.22μm filter head, and the concentration of U(VI) in the solution was determined at 652nm using an ultraviolet spectrophotometer, and the color developer was arsenazo III;

[0058] The reduction effect of MoS2 on U(VI) after ultrasonic time at different piezoelectric catalyst dosages is shown in Figure 2. Figure 4 As shown, the reduction efficiencies calculated by substituting into the formula are 66.3%, 85.8%, 80.5%, 74.9% and 60.1%, respectively.

[0059] Example 4: Weigh 5 portions of 100 mL of a 5 mg / L U(VI) solution, adjust the solution pH to 2.9, 5, 7, 9, and 11 using dilute hydrochloric acid or sodium hydroxide, add 100 mg of molybdenum disulfide, and stir the reaction system in the dark for 20 min to reach adsorption-desorption equilibrium before reacting;

[0060] The ultrasonic generator was turned on for reaction, the ultrasonic frequency was 40kHz, the ultrasonic power was 300W, U(VI) was reduced by piezoelectric catalysis, the ultrasonic reaction time was 20min, samples were taken at regular intervals, filtered with a 0.22μm filter head, and the concentration of U(VI) in the solution was determined at 652nm using an ultraviolet spectrophotometer, and the color developer was arsenazo III;

[0061] The reduction effect of MoS2 on U(VI) after ultrasound time under different pH conditions is shown in Figure 2. Figure 5 As shown, the reduction efficiencies calculated by substituting into the formula are 88.1%, 59.5%, 41.9%, 45.6% and 18.8%, respectively.

[0062] Example 5: Weigh 5 portions of 100 mL of a 5 mg / L U(VI) solution, adjust the solution pH to 2.9 using dilute hydrochloric acid or sodium hydroxide, add 100 mg of molybdenum disulfide, and stir the reaction system in the dark for 20 min to reach adsorption-desorption equilibrium before reacting;

[0063] The ultrasonic generator was turned on for reaction, the ultrasonic frequency was 40kHz, the ultrasonic power was 40W, 80W, 160W, 240W, and 300W respectively, U(VI) was reduced by piezoelectric catalysis, the ultrasonic reaction time was 20min, samples were taken at regular intervals, filtered with a 0.22μm filter head, and the U(VI) concentration in the solution was determined at 652nm by an ultraviolet spectrophotometer, and the color developer was arsenazo III;

[0064] The reduction effect of MoS2 on U(VI) under different ultrasonic powers is shown in Figure 2. Figure 6 As shown, the reduction efficiencies calculated by substituting into the formula are 41.8%, 58.6%, 67.9%, 75.5% and 87.3%, respectively.

[0065] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis. It is characterized in that The method comprises the following steps: at room temperature, wastewater containing U(VI) is placed in a reactor, a piezoelectric catalyst is added, and after reaching adsorption-desorption equilibrium under dark conditions, U(VI) is reduced under ultrasonic driving.

2. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that The piezoelectric catalyst is barium titanate or molybdenum disulfide.

3. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 2, It is characterized in that The dosage of the piezoelectric catalyst is 0.5-2.5 g / L.

4. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that The concentration range of U(VI) in the treatment system is 2.0-15 mg / L.

5. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that In the treatment system, the external mechanical force used is low-frequency ultrasound with a frequency of 40kHz and a power of 40-300W.

6. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that The initial pH value of the solution reaction in the treatment system is 2.8-11.

7. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that The piezoelectric catalyst is pretreated before use, including cleaning, drying and activation steps.

8. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that In the reduction reaction of the piezoelectric catalyst driven by ultrasound, methanol is added as a hole inhibitor to adjust the separation efficiency of the piezoelectric electron-hole pairs.

9. The method for high-efficiency reduction of U(VI) in water by low-frequency ultrasound-driven piezoelectric catalysis according to claim 1, It is characterized in that After completing a reduction reaction, the piezoelectric catalyst is regenerated by a physical or chemical method.

Citation Information

Patent Citations

  • Lamellar nanometer barium titanate and preparation method thereof, and applications in sewage treatment based on piezoelectric photocatalysis

    CN110465282A

  • Method for efficiently reducing and recycling precious metal in leachate through piezoelectric photocatalysis process

    CN113832354A

  • Synthesis method and piezoelectric catalysis application of Z-type semiconductor / covalent organic framework heterojunction

    CN118562145A

Cited By

  • Application of molybdenum disulfide-based piezoelectric catalytic material in extraction of uranium from seawater

    CN121422990A