Thermal environment barrier coating, preparation method thereof and high-temperature-resistant component
Through the combination of rare earth silicate dense layer and high-entropy ceramic feather columnar structure, the problem of insufficient anti-water oxygen corrosion ability of thermal environment barrier coating in high-temperature water oxygen environment is solved, and higher anti-water oxygen protection and isolation are achieved Thermal effect.
Patent Information
- Application Number
- CN202411272521.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The existing thermal environment barrier coatings lack the ability to resist water oxygen corrosion in high-temperature water oxygen corrosion environments, and are prone to cracks and holes, resulting in rapid degradation and failure.
Using a combined structure of rare earth silicate dense layer and high strain tolerance layer, prepared by PS-PVD technology, the rare earth silicate dense layer is combined with a high entropy ceramic feather columnar structure to form a high density and high strain tolerance heat. Environmental barrier coating reduces the difference in thermal expansion coefficient and thermal mismatch stress, and improves the resistance to water and oxygen corrosion.
It significantly improves the anti-water oxygen corrosion performance of thermal environment barrier coatings, extends the service life, reduces the degradation rate and failure probability in high-temperature water oxygen environments, and enhances the overall thermal insulation effect.
Smart Images

Figure CN119019186A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of high-temperature protective coatings, and in particular relates to a thermal environment barrier coating and a preparation method thereof, and a high-temperature resistant component. Background Art
[0002] High-temperature alloys are currently the most widely used and mature materials for high-temperature structural components of aircraft engines. They have the characteristics of high temperature resistance, oxidation resistance, corrosion resistance and fatigue resistance, as well as high high-temperature strength, creep strength and endurance strength. With the development of the aviation industry and gas turbines, components such as turbine blades will be subjected to higher temperatures, and high-temperature alloys are no longer applicable. Therefore, seeking a new type of high-temperature resistant material has become a new demand.
[0003] Ceramic matrix composites (CMC) have low density (about 1 / 3 of high temperature alloys), high specific strength, high specific modulus, and excellent high temperature thermodynamic properties. Compared with high temperature alloys, CMC has excellent resistance to high temperature oxidation and creep, and has a certain ability to resist crack propagation. It is a promising choice to replace high temperature alloys as a new matrix. Silicon carbide ceramics and related composite materials have low density, only 20%-30% of high temperature alloys; strong performance designability, mechanical properties and thermal conductivity can be significantly improved with the increase of fiber content; excellent high temperature mechanical properties, strength does not decrease significantly with temperature increase; high fatigue limit, up to 90% of static strength; and excellent anti-oxidation, corrosion resistance, and wear resistance. It is regarded as the main candidate material for high temperature components of the new generation of high thrust-to-weight ratio aircraft engines. In the water-oxygen fuel gas application environment, silicon carbide ceramic materials undergo rapid performance degradation due to high temperature water vapor corrosion. Therefore, the research on silicon carbide ceramic materials and high temperature protection technology is of great significance for my country's future high thrust-to-weight ratio aircraft engines.
[0004] Environmental barrier coating (EBC) is an indispensable surface protective coating for ceramic materials. It can establish a barrier between high-temperature structural materials and the harsh environment of the engine (corrosive media, high-speed airflow scouring, etc.), preventing or reducing the impact of the engine environment on the performance of high-temperature structural materials. The rare earth silicate system, which is widely recognized as an environmental barrier coating material, has good resistance to water and oxygen corrosion. Taking ytterbium disilicate (Yb2Si2O7) as an example, this material system has excellent resistance to water and oxygen corrosion under quasi-static conditions. However, in the actual service environment where the water and oxygen corrosive medium flows rapidly, material loss, pores and microcracks will occur, which will reduce its resistance to water and oxygen.
[0005] The thermal barrier coating formed by combining thermal barrier coating and environmental barrier coating is the latest generation of high temperature protection coating system. Guo Hongbo's team at Beijing University of Aeronautics and Astronautics prepared Si bonding layer and Yb 2 SiO 5The YbSiO2 intermediate layer was prepared by PS-PVD technology (Gd 0.9 Yb 0.1 ) 2 Zr 2 O 7 The surface layer is formed into a thermal barrier coating system, and its overall anti-sintering performance is studied at 1300℃ and 1400℃. However, the thermal expansion coefficients of ytterbium monosilicate and SiC are quite different in this study, which is easy to cause cracks due to thermal mismatch stress, thus forming water-oxygen corrosion channels. In addition, there are a large number of microcracks between the layered structures prepared by APS technology. The presence of microcracks provides channels for water-oxygen corrosion, which is not conducive to water-oxygen corrosion protection. Similarly, the team prepared Hf by APS technology. 0.84 Y 0.16 O 1.92 / Yb 2 SiO 5 / Si thermal barrier coating system and carried out oxidation experiments at 1300℃ for up to 100h. 0.84 Y 0.16 O 1.92 Surface layer and Yb 2 SiO 5 There are a lot of micro cracks and pores between the layers in the middle layer, which is not conducive to water and oxygen corrosion protection. The team led by Cao Xueqiang of Wuhan University of Technology used APS technology to prepare LaMgAl 11 O 19 / Yb 2 Si 2 O 7 / Si thermal barrier coating system and conducted water-oxygen corrosion research at 1300℃. However, due to the presence of a large number of interlaminar microcracks and pore structures in the thermal barrier surface layer and environmental barrier intermediate layer prepared by APS technology, vertical cracks or through-crack structures appeared in the thermal barrier coating during the heat preservation heat treatment stage after spraying and before the water-oxygen corrosion experiment, providing a rapid diffusion channel for the water-oxygen corrosion medium. A large number of through-cracks appeared after 60h of water-oxygen corrosion at 1300℃. Similarly, the team prepared LaMgAl by APS technology. 11 O 19 / Yb 2 SiO 5 / Si thermal barrier coating system and the oxidation behavior was studied at 1300℃. 11 O 19 and Yb 2 SiO 5 There is a large difference in thermal expansion coefficient between them and SiC. There are a large number of through cracks inside the sprayed coating. After 50-100 hours of oxidation, the opening displacement of the through crack tips increases significantly, which will provide a rapid diffusion channel for water and oxygen corrosive media.
[0006] The coating system of AECC Beijing Institute of Aeronautical Materials (CN 116253584 B) is Yb 2 O 3 -Y 2 O 3 -HfO 2 Ternary oxide surface layer / Yb 2 Si 2 O 7 -Yb 2 SiO 5 Doped interlayer / R-Al-Si-O glass-ceramic bonding layer, in which the gradient Yb 2 Si 2 O 7 -Yb2SiO 5 The APS technology also has the problem of many pores and insufficient water and oxygen protection. 2 SiO 5 The overall thermal expansion coefficient is increased, resulting in greater thermal mismatch stress. In addition, the adhesive layer prepared by the slurry method leads to a low overall bonding strength of the coating. The Institute of Aerospace Special Materials and Process Technology (CN 109336647 B) uses VPS technology to prepare HfO 2 / HfO 2 -Yb 2 SiO 5 Doping / Yb 2 SiO 5 / Si thermal barrier coating system, because the hafnium oxide surface layer prepared by VPS technology does not have a high strain tolerance structure, it has problems such as insufficient thermal barrier performance, and the introduction of Yb 2 SiO 5 The overall thermal expansion coefficient is increased, resulting in greater thermal mismatch stress. Summary of the invention
[0007] In view of the problem that existing thermal environment barrier coatings have insufficient resistance to water and oxygen corrosion, the present invention provides a thermal environment barrier coating and a preparation method thereof, and a high temperature resistant component.
[0008] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0009] In one aspect, the present invention provides a thermal environment barrier coating, comprising a dense layer and a high strain tolerance layer, wherein the dense layer comprises rare earth silicate, and the high strain tolerance layer comprises high entropy ceramic.
[0010] Optionally, the high strain tolerance layer includes a plurality of feather columnar structures arranged on the surface of the dense layer, and the feather columnar structures are composed of the high entropy ceramic.
[0011] Optionally, the high entropy ceramic comprises (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 .
[0012] Optionally, the rare earth silicate includes one or more of rare earth monosilicates and rare earth disilicates, and the rare earth elements of the rare earth silicate include one or more of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, yttrium and erbium.
[0013] Optionally, the rare earth silicate is selected from rare earth double silicate, and the rare earth double silicate includes Yb 2 Si 2 O 7 .
[0014] Optionally, the thickness of the dense layer is 75-200 μm.
[0015] Optionally, the high strain tolerance layer has a thickness of 150-300 μm.
[0016] Optionally, a Si layer is further included, wherein the Si layer is used for contacting the substrate, the Si layer is located on a side of the dense layer away from the high strain tolerance layer, and the thickness of the Si layer is 50-150 μm.
[0017] In yet another aspect, the present invention provides a high temperature resistant component, comprising a substrate and the thermal environment barrier coating as described above disposed on the substrate, wherein the substrate is selected from SiC.
[0018] In another aspect, the present invention provides a method for preparing the thermal environment barrier coating as described above, comprising the following steps:
[0019] Using rare earth silicates as raw materials, the dense layer is deposited;
[0020] A high entropy ceramic is deposited on the surface of the dense layer to form a high strain tolerance layer.
[0021] Optionally, the method further includes: using SiC as a substrate, depositing a Si layer on the substrate, and forming the dense layer on the Si layer.
[0022] Optionally, the Si layer, the dense layer and the high strain tolerance layer are all prepared by using PS-PVD technology.
[0023] Optionally, the PS-PVD preparation parameters of the Si layer are: spraying current of 1500-1700A, argon flow rate of 100-120NLPM (standard liters per minute), hydrogen flow rate of 4-7NLPM (standard liters per minute), and cabin pressure of 35-50mbar; and / or
[0024] The PS-PVD preparation parameters of the dense layer are: spraying current of 2400-2600A, argon flow rate of 90-110 NLPM (standard liters per minute), helium flow rate of 15-30 NLPM (standard liters per minute), and chamber pressure of 1.2-2.0 mbar; and / or
[0025] The PS-PVD preparation parameters of the high strain tolerance layer are: the current is controlled at 2400-2600A, the argon flow rate is 25-45 NLPM (standard liters per minute), and the helium flow rate is 50-70 NLPM (standard liters per minute).
[0026] Optionally, after the dense layer is sprayed, the sprayed dense layer is heat treated at a temperature of 1250 to 1350° C. and for a time of 2 to 10 hours.
[0027] According to the thermal environment barrier coating provided by the present invention, rare earth silicate is used as a high-density layer, which can block the corrosion of high-temperature water and oxygen on the substrate, and achieves good matching with the substrate through the intrinsic low thermal expansion coefficient of the material, avoiding excessive thermal mismatch stress, thereby making it possible to prepare a high-density structure. The high-density structure is used to further improve the water-oxygen corrosion resistance by avoiding holes or microcracks to form a fast water-oxygen diffusion channel; at the same time, in order to avoid the rapid flow of water-oxygen mixed gas from scouring the high-density layer and causing rapid degradation of the material and structure, the present invention uses high-entropy ceramics in the high A high strain tolerance layer is formed on the surface of the dense layer, which can not only provide excellent anti-water and oxygen corrosion protection through the intrinsic high water and oxygen activation energy of the material, but also significantly reduce the gas flow rate near the high dense layer, thereby avoiding the direct contact between the fast-flowing water and oxygen mixed gas and the rare earth silicate, which leads to rapid degradation of the material and structure. It can also reduce the thermal mismatch stress of the surface layer through the high strain tolerance structure, thereby avoiding premature spalling and failure of the surface layer. In addition, it can also reduce the intrinsic thermal conductivity of the material through the high entropy effect, thereby further improving the overall thermal insulation effect of the coating system and reducing the degradation rate and failure probability of the high dense layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the structure of the thermal environment barrier coating provided by the present invention;
[0029] Figure 2 This is a cross-sectional morphology of the thermal environment barrier coating prepared in Example 1;
[0030] Figure 3This is a cross-sectional morphology of the target thermal environment barrier coating prepared in Example 2 after 50 hours of water-oxygen corrosion;
[0031] Figure 4 This is a cross-sectional morphology of the environmental barrier coating prepared in Comparative Example 2 after 50 hours of water-oxygen corrosion;
[0032] Figure 5 This is a cross-sectional morphology of the target thermal environment barrier coating prepared in Example 3 after 150 hours of water-oxygen corrosion;
[0033] Figure 6 This is a cross-sectional morphology of the environmental barrier coating prepared in Comparative Example 3 after 150 hours of water-oxygen corrosion;
[0034] Figure 7 This is a cross-sectional morphology of the target thermal environment barrier coating prepared in Example 4 after 300 hours of water-oxygen corrosion;
[0035] Figure 8 This is a cross-sectional morphology of the environmental barrier coating prepared in Comparative Example 4 after 300 hours of water-oxygen corrosion;
[0036] Fig. 9 The SiO2 in the sprayed state or after water-oxygen corrosion of Examples 2, 3, 4 and Comparative Examples 2, 3, 4 is shown in FIG. 2 Thickness plot of thermally grown oxide;
[0037] The reference numerals in the drawings of the specification are as follows:
[0038] 1. Substrate; 2. Si layer; 3. Dense layer; 4. High strain tolerance layer. DETAILED DESCRIPTION
[0039] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] In the present invention, when a layer is described as being "on" or "over" another layer or substrate, it should be understood that unless explicitly stated to the contrary, these layers can be directly in contact with each other or have another layer or feature between the layers. Therefore, these terms simply describe the relative position of the layers to each other and do not necessarily mean "above", as the relative position of above or below depends on the orientation of the device relative to the viewer.
[0041] See also Figure 1 As shown, an embodiment of the present invention provides a thermal environment barrier coating, including a dense layer 3 and a high strain tolerance layer 4, wherein the dense layer 3 includes rare earth silicate, and the high strain tolerance layer 4 includes high entropy ceramics.
[0042] In the thermal environment barrier coating, rare earth silicate is used as the high-density layer 3, which can block the corrosion of high-temperature water and oxygen on the substrate 1. The low thermal expansion coefficient of the material is used to achieve a good match with the substrate 1, avoiding excessive thermal mismatch stress, thereby making it possible to prepare a high-density structure. The high-density structure is used to further improve the water-oxygen corrosion resistance by avoiding holes or microcracks to form a fast water-oxygen diffusion channel; at the same time, in order to avoid the rapid flow of water-oxygen mixed gas from scouring the high-density layer 3 and causing rapid degradation of the material and structure, the present invention uses high-entropy ceramics in the high-density layer A high strain tolerance layer 4 is formed on the surface of 3, which can not only provide excellent anti-water and oxygen corrosion protection through the intrinsic high water and oxygen activation energy of the material, but also significantly reduce the gas flow rate near the high-density layer 3, thereby avoiding the rapid degradation of the material and structure caused by the direct contact between the fast-flowing water and oxygen mixed gas and the rare earth silicate, but also reduce the thermal mismatch stress of the surface layer through the high strain tolerance structure, thereby avoiding premature peeling and failure of the surface layer. In addition, the intrinsic thermal conductivity of the material can be reduced through the high entropy effect, thereby further improving the overall thermal insulation effect of the coating system and reducing the degradation rate and failure probability of the high-density layer 3.
[0043] In some embodiments, the high strain tolerance layer 4 includes a plurality of feather columnar structures arranged on the surface of the dense layer 3 , and the feather columnar structures are composed of the high entropy ceramic.
[0044] In the description of the present invention, the term "feather-like structure" refers to slender columnar crystals similar to feathers, which grow on the surface of the dense layer 3 in a direction perpendicular to the surface of the dense layer 3 and show obvious directional arrangement characteristics. The crystals are not completely fitted together, and gaps are retained to achieve their high strain tolerance.
[0045] The feather columnar structure formed by the high entropy ceramic can provide a high strain tolerance, so that the rare earth silicate and the high entropy ceramic with a large CTE difference can be well combined without generating a microcrack structure. The high strain tolerance enables the high entropy ceramic layer to better cope with the impact of the thermal mismatch stress in the surface during the thermal cycle, reduce the thermal mismatch stress of the surface layer, and is not easy to generate vertical cracks and other structures, thereby reducing the risk of premature peeling and improving the thermal cycle life. At the same time, the feather columnar structure can reduce the surface high-temperature water and oxygen flow rate in a fast-flowing high-temperature water and oxygen environment, and as an environmental barrier layer of the dense layer 3, it provides water and oxygen protection for the dense layer 3, solving the problem of insufficient protection of rare earth silicates in a dynamic water and oxygen environment.
[0046] In some embodiments, the height of the feather-like structure is 150-300 μm.
[0047] In some embodiments, the high entropy ceramic comprises a rare earth zirconate.
[0048] Rare earth zirconate high entropy ceramics have excellent thermal stability and resistance to water, oxygen and molten salt corrosion, and can provide additional water and oxygen protection for thermal environment barrier coatings.
[0049] In a preferred embodiment, the high entropy ceramic comprises (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 .
[0050] (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 The intrinsic properties of the high water-oxygen activation energy and low thermal conductivity make the high strain tolerance layer 4 have good high temperature stability in a high-velocity water-oxygen environment, thereby separating the dense layer 3 of rare earth silicate from high-velocity water vapor, significantly reducing the gas flow rate near the dense layer 3, thereby avoiding direct contact between the fast-flowing water-oxygen mixed gas and the dense layer 3, resulting in rapid degradation of the material and structure. And (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 By enhancing phonon scattering through the high entropy effect and thus having a low intrinsic thermal conductivity, the overall thermal insulation effect of the coating system can be increased, which is of great significance for increasing the operating temperature of engines, reducing fuel consumption, and improving thrust-to-weight ratio.
[0051] In some embodiments, the rare earth silicate includes one or more of rare earth monosilicates and rare earth disilicates, and the rare earth elements of the rare earth silicate include one or more of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, yttrium and erbium.
[0052] In some embodiments, the dense layer 3 is a single layer or a multilayer. When the dense layer 3 is a single layer, the dense layer 3 may include a single rare earth silicate or multiple rare earth silicates; when the dense layer 3 is a multilayer, each of the dense layers 3 independently includes a single rare earth silicate or multiple rare earth silicates, and the materials of the multilayer dense layers 3 may be the same or different.
[0053] In a preferred embodiment, the dense layer 3 is a single layer of rare earth silicate.
[0054] In a preferred embodiment, the rare earth silicate is selected from rare earth double silicate, and the rare earth double silicate includes Yb 2 Si 2 O 7 .
[0055] Ytterbium disilicate (Yb 2 Si 2 O 7 ) has excellent resistance to water and oxygen corrosion in a quasi-static corrosion environment; compared with ytterbium monosilicate with a higher thermal expansion coefficient, its thermal expansion coefficient is close to that of SiC, which is an intrinsic property of the material, making it possible to prepare a high-density layered structure on the SiC substrate 1. The high-density layered structure is beneficial to improving protection and reducing the generation of various corrosion channels.
[0056] Theoretically, in the dense layer 3, Yb 2 Si 2 O 7 The purity of Yb should be as high as possible, but due to the limitations of raw material purity, synthesis process and preparation process, the presence of a certain amount of impurities or by-products is allowed without affecting its function. For example, in some embodiments, in the dense layer 3, Yb 2 Si 2 O 7 The mass content of Yb is 90% or more. Preferably, in the dense layer 3, Yb 2 Si 2 O 7 The mass content of Yb is 93% or more. More preferably, in the dense layer 3, Yb 2 Si 2 O 7 The quality content is 96% and above.
[0057] In some embodiments, the dense layer 3 has a thickness of 75 to 200 μm.
[0058] If the thickness of the dense layer 3 is too low, its protective effect is limited, and it is easy to form holes or microcracks connected to the substrate 1 in a high-temperature water and oxygen environment, affecting the protective effect on the substrate 1.
[0059] In some embodiments, the high strain tolerance layer 4 has a thickness of 150-300 μm.
[0060] The thickness of the high strain tolerance layer 4 is related to the height of the feather columnar structure. Generally, the columnar heights of the feather columnar structure vary. The thickness of the high strain tolerance layer 4 is determined by the height of the higher column in the feather columnar structure.
[0061] If the thickness of the high strain tolerance layer 4 is too low, it is easy to be worn out in a long-term water-oxygen corrosion environment, resulting in exposure of the dense layer 3 , and the protective effect of the dense layer 3 is reduced.
[0062] In some embodiments, the thermal barrier coating further includes a Si layer 2, which is used to contact the substrate 1. The Si layer 2 is located on the side of the dense layer 3 away from the high strain tolerance layer 4, and the thickness of the Si layer 2 is 50-150 μm.
[0063] The Si layer 2 is located between the substrate 1 and the dense layer 3, and acts as a bonding layer. The bonding between the Si layer 2 and the substrate 1 affects the bonding performance of the thermal barrier coating system. From the perspective of material design, the Si used in the present invention has a thermal expansion coefficient similar to that of the SiC substrate 1, and the two have the characteristics of high compatibility, low thermal mismatch stress, etc., which improves the bonding performance of the coating system.
[0064] In some embodiments, a thermally grown oxide layer is formed on a side of the Si layer 2 facing away from the substrate 1 .
[0065] The thermally grown oxide layer is formed by the reaction between the Si layer 2 and water oxygen under high temperature conditions during the long-term protection of the substrate 1 . The formed thermally grown oxide layer has certain barrier properties and avoids oxidation of the substrate 1 .
[0066] In some optional embodiments, hafnium oxide is disposed on a side of the Si layer 2 facing away from the substrate 1 .
[0067] Another embodiment of the present invention provides a high temperature resistant component, comprising a substrate and the thermal environment barrier coating as described above disposed on the substrate.
[0068] Exemplary applications of the high temperature resistant components include turbine components, specifically, those located in the compressor section (e.g., compressor blades, blades and / or shrouds), combustion section (e.g., combustor, liner and / or heat shield), or turbine section (e.g., turbine blades, blades and / or shrouds). Application scenarios of the turbine components include high bypass turbofan jet engines, turbojet engines, turboprop engines or turboshaft gas turbine engines, as well as industrial and marine gas turbine engines and auxiliary power units.
[0069] In one embodiment, the substrate is selected from SiC.
[0070] Another embodiment of the present invention provides a method for preparing the thermal environment barrier coating as described above, comprising the following steps:
[0071] Using rare earth silicates as raw materials, the dense layer is deposited;
[0072] A high entropy ceramic is deposited on the surface of the dense layer to form a high strain tolerance layer.
[0073] The present invention uses highly dense rare earth silicates and high-entropy ceramics with high strain tolerance to form a thermal barrier coating, which can effectively reduce the problems of the thermal barrier coating being prone to crack channels and water-oxygen corrosion failure caused by direct contact with water and oxygen, thereby achieving the effect of increasing the overall resistance to water-oxygen corrosion. The introduction of low thermal conductivity high-entropy ceramics not only increases the overall resistance to water-oxygen corrosion, but also can further increase the overall thermal insulation effect, thereby improving the engine's efficiency.
[0074] In some embodiments, the preparation method further includes: using SiC as a substrate, depositing a Si layer on the substrate, and forming the dense layer on the Si layer.
[0075] In some embodiments, the Si layer, the dense layer and the high strain tolerance layer are prepared by one or more methods selected from the group consisting of plasma spraying, thermal spraying, ion plasma deposition, physical vapor deposition, chemical vapor deposition and atomic layer deposition.
[0076] In a preferred embodiment, the Si layer, the dense layer and the high strain tolerance layer are all prepared by using PS-PVD technology.
[0077] Compared with other existing preparation methods, the Si layer and dense layer prepared by the PS-PVD technology in the present invention have a highly dense layered structure. Among them, the dense Si can effectively prevent oxygen from oxidizing the SiC substrate in a high-temperature environment, thereby increasing the bonding performance of the coating system and the protective performance of the SiC substrate. The dense layer of the high-density layered structure improves the water and oxygen protection ability by avoiding holes and microcracks to form a fast water and oxygen diffusion channel. Compared with other preparation technologies, such as APS technology, the rare earth silicate dense layer prepared by PS-PVD technology avoids the formation of holes or microcracks and significantly improves the density, and the water and oxygen protection effect is better.
[0078] PS-PVD technology combines the characteristics of APS and EB-PVD technologies, and can efficiently deposit a high strain tolerance layer of a feather columnar structure and a dense layer of a high-density layered structure. The high strain tolerance of the feather columnar structure can reduce the impact of the difference in the coefficient of thermal expansion (CTE), and the high-density layered structure is conducive to improving protection and reducing the generation of various corrosion channels.
[0079] In some embodiments, the PS-PVD preparation parameters of the Si layer are: spraying current is 1500-1700A, argon flow rate is 100-120NLPM (standard liters per minute), hydrogen flow rate is 4-7NLPM (standard liters per minute), and cabin pressure is 35-50mbar.
[0080] In some embodiments, the PS-PVD preparation parameters of the dense layer are: spraying current is 2400-2600A, argon flow rate is 90-110NLPM (standard liters per minute), helium flow rate is 15-30NLPM (standard liters per minute), and cabin pressure is 1.2-2.0mbar.
[0081] When using the spray parameters as described above, Si and Yb can be made 2 Si 2 O 7 The powder is fully melted to form a liquid phase spraying mechanism to prepare a highly dense layered structure of Si and Yb 2 Si 2 O 7 layer.
[0082] In some embodiments, the PS-PVD preparation parameters of the high strain tolerance layer are: the current is controlled at 2400-2600A, the argon flow rate is 25-45 NLPM (standard liters per minute), and the helium flow rate is 50-70 NLPM (standard liters per minute).
[0083] The spraying parameters described above enable the spraying to proceed in a gas-liquid-solid multiphase deposition mechanism to produce a feather-like structure with high strain tolerance. The high strain tolerance structure can reduce the thermal mismatch stress of the high entropy ceramic, thereby reducing the risk of premature spalling.
[0084] In some embodiments, after the dense layer is sprayed, the sprayed dense layer is heat treated at a temperature of 1250 to 1350° C. for a time of 2 to 10 hours.
[0085] During the heat treatment process, the heating and cooling rate is 5°C / min.
[0086] Through Yb 2 Si 2 O 7 Continuing heat treatment of the layer can make Yb 2 Si 2 O 7 The micro cracks in the layer heal and reduce the internal amorphous Yb 2 SiO 5 , avoid Yb 2 SiO 5 The difference in thermal expansion coefficient between SiC and SMT leads to the generation of micro cracks.
[0087] In some embodiments, the substrate is surface treated before the Si layer is formed.
[0088] The surface treatment includes one or more of ultrasonic cleaning, organic solvent cleaning, surface roughening treatment, chemical treatment, heat treatment, plasma treatment and laser treatment.
[0089] The surface roughening treatment includes one or more of sandblasting and mechanical grinding.
[0090] The chemical treatment includes one or more of an acid treatment and an alkali treatment.
[0091] Surface treatment is used to remove impurities from the substrate surface and increase the bonding strength with other layers.
[0092] The present invention is further described below by way of examples.
[0093] Example 1
[0094] This embodiment is used to illustrate the thermal environment barrier coating and the preparation method thereof disclosed in the present invention, including the following steps:
[0095] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0096] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 450 mm, a spraying temperature of 650-800 °C, a spray gun speed of 500 mm / s, a spraying current of 1650 A, an argon flow rate of 110 NLPM (standard liters per minute), and a hydrogen flow rate of 6 NLPM;
[0097] S3. Preparation of Yb using PS-PVD technology 2 Si 2 O 7 layer, the spraying distance is 950mm, the spraying temperature is controlled at 900-1100℃, the spraying gun travel is 800mm / s, the spraying current is controlled at 2600A, the argon flow rate is controlled at 100NLPM, and the helium flow rate is controlled at 20NLPM;
[0098] S4. After spraying Yb 2 Si 2 O 7 After the layer, the sample was taken out and kept in an air atmosphere at 1300 °C for 3 hours with a heating and cooling rate of 5 °C / min;
[0099] S5. Prepared by PS-PVD technology (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7For the high entropy ceramic layer, the spraying distance is controlled at 1000mm, the spraying temperature is controlled at 900-1100℃, the spraying speed is 500mm / s, the current is controlled at 2600A, the argon flow rate is controlled at 35NLPM, and the helium flow rate is controlled at 60NLPM to obtain the target thermal environment barrier coating.
[0100] The thermal barrier coating was polished and its cross section was observed by electron microscope. The results are as follows: Figure 2 As shown by Figure 2 It can be seen that the Si layer and Yb 2 Si 2 O 7 The layers are dense structures, while the high entropy ceramic layer is a high strain tolerance layer with a feather-like structure.
[0101] Comparative Example 1
[0102] This comparative example is used to compare and illustrate the thermal environment barrier coating and its preparation method disclosed in the present invention. The preparation method is the implementation steps of Example 1 except for the preparation part of the high entropy ceramic layer, that is, S1 to S4 in Example 1, and specifically includes the following steps:
[0103] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0104] S2. Si was prepared by PS-PVD technology, with a spraying distance of 450 mm, a spraying temperature of 650-800 °C, a spray gun speed of 500 mm / s, a spraying current of 1650 A, an argon flow rate of 110 NLPM (standard liters per minute), and a hydrogen flow rate of 6 NLPM;
[0105] S3. Using Yb 2 Si 2 O 7 Technology for preparing Yb 2 Si 2 O 7 layer, the spraying distance is 950mm, the spraying temperature is controlled at 900-1100℃, the spraying gun travel is 800mm / s, the spraying current is controlled at 2600A, the argon flow rate is controlled at 100NLPM, and the helium flow rate is controlled at 20NLPM;
[0106] S4. After spraying Yb 2 Si 2 O 7 After coating, the sample was taken out and kept at 1300°C in air atmosphere for 3 hours with a heating and cooling rate of 5°C / min to obtain the target thermal environment barrier coating.
[0107] Performance Testing
[0108] The thermal barrier coatings prepared in Example 1 and Comparative Example 1 were measured by scanning electron microscopy to measure Yb 2 Si 2 O 7 After measuring the thickness of the oxide layer on the Si layer and the oxide layer on the Si layer, the test results are filled in Table 1.
[0109] Table 1
[0110]
[0111] It can be seen from the test results in Table 1 that no obvious thermally grown oxides appear in Example 1 and Comparative Example 1 after heat treatment, which is consistent with the 2 Si 2 O 7 The density of the layer is related to the density of the Yb 2 Si 2 O 7 The layer adds protection to the interior.
[0112] Example 2
[0113] This embodiment is used to illustrate the thermal environment barrier coating and the preparation method thereof disclosed in the present invention, including the following steps:
[0114] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0115] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 500 mm, a spraying temperature of 650-800 °C, a spray gun speed of 450 mm / s, a spraying current of 1550 A, an argon gas of 120 NLPM (standard liters per minute), and a hydrogen gas of 7 NLPM;
[0116] S3. Preparation of Yb 2 Si 2 O 7 layer, the spraying distance is 900mm, the spraying temperature is controlled at 900-1100℃, the spraying gun travel speed is 750mm / s, the spraying current is controlled at 2500A, the argon flow rate is 110NLPM, and the helium flow rate is 25NLPM;
[0117] S4. After spraying Yb 2 Si 2 O 7 After the layer, the sample was taken out and kept in an air atmosphere at 1300 °C for 3 hours with a heating and cooling rate of 5 °C / min;
[0118] S5. Prepared by PS-PVD technology (Y 0.2 La0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 For the high entropy ceramic layer, the spraying distance is controlled at 950mm, the spraying temperature is controlled at 900-1100℃, the spraying speed is 450mm / s, the current is controlled at 2600A, the argon flow rate is 35NLPM, and the helium flow rate is 60NLPM to obtain the target thermal environment barrier coating.
[0119] Comparative Example 2
[0120] This comparative example is used to compare and illustrate the thermal environment barrier coating and its preparation method disclosed in the present invention. The preparation method is the implementation steps of Example 2 except for the preparation part of the high entropy ceramic layer, that is, S1 to S4 in Example 2, and specifically includes the following steps:
[0121] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0122] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 500 mm, a spraying temperature of 650-800 °C, a spray gun speed of 450 mm / s, a spraying current of 1550 A, an argon gas of 120 NLPM (standard liters per minute), and a hydrogen gas of 7 NLPM;
[0123] S3. Preparation of Yb 2 Si 2 O 7 layer, the spraying distance is 900mm, the spraying temperature is controlled at 900-1100℃, the spraying gun travel speed is 750mm / s, the spraying current is controlled at 2500A, the argon flow rate is 110NLPM, and the helium flow rate is 25NLPM;
[0124] S4. After spraying Yb 2 Si 2 O 7 After coating, the sample was taken out and kept at 1300°C in air atmosphere for 3 hours with a heating and cooling rate of 5°C / min to obtain the target thermal environment barrier coating.
[0125] Performance Testing
[0126] The thermal environment barrier coating prepared in Example 2 and Comparative Example 2 was subjected to a water-oxygen corrosion test in a 1400°C water-oxygen environment. The experimental conditions were: atmospheric atmosphere, a 1700X tube furnace was used to control the sample temperature to 1400°C ± 2°C, a 1600°C thermocouple was used to measure the temperature and feedback to adjust the tube furnace setting temperature, a water vapor flow rate of 23.2 g / min, introduced from one side of the tube furnace, and the other side of the tube furnace was connected to the atmosphere, and the water-oxygen corrosion time was 50 h. After the water-oxygen corrosion, the cross-section was observed, and the test results obtained were as follows: Figure 3 and Figure 4 As shown, the test remaining Yb 2 Si 2 O 7 The layer thickness and the Si layer thermally grown oxide thickness, the test results are filled in Table 2.
[0127] Table 2
[0128]
[0129] Depend on Figure 3 , Figure 4 As can be seen from the test results in Table 2, the Yb 2 Si 2 O 7 The surface of the layer was obviously corroded, and the surface flatness decreased; in Example 2, Yb 2 Si 2 O 7 The remaining thickness of the layer is significantly higher than that of the comparative example 2, and the thickness of the thermally grown oxide of the Si layer in the embodiment 2 is significantly lower than that of the comparative example 2, indicating that the high entropy ceramic layer with feather columnar structure can effectively 2 Si 2 O 7 The protective effect of the layer reduces the Yb 2 Si 2 O 7 Corrosion of Si layer and Si layer in high temperature water and oxygen environment.
[0130] Example 3
[0131] This embodiment is used to illustrate the thermal environment barrier coating and the preparation method thereof disclosed in the present invention, including the following steps:
[0132] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0133] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 500 mm, a spraying temperature of 650-800 °C, a spray gun speed of 500 mm / s, a spraying current of 1600 A, argon gas of 115 NLPM (standard liters per minute), and hydrogen gas of 5 NLPM;
[0134] S3. Preparation of Yb 2 Si 2 O 7 layer, the spraying distance is 900mm, the spraying temperature is controlled at 900-1100℃, the spraying gun travel is 700mm / s, the spraying current is controlled at 2550A, the argon flow rate is 95NLPM, and the helium flow rate is 30NLPM;
[0135] S4. After spraying Yb 2 Si 2 O 7 After the layer, the sample was taken out and kept in an air atmosphere at 1300 °C for 3 hours with a heating and cooling rate of 5 °C / min;
[0136] S5. Prepared by PS-PVD technology (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 For the high entropy ceramic layer, the spraying distance is controlled at 1000mm, the spraying temperature is controlled at 900-1100℃, the spraying speed is 400mm / s, the current is controlled at 2550A, the argon flow rate is 40NLPM, and the helium flow rate is 70NLPM to obtain the target thermal environment barrier coating.
[0137] Comparative Example 3
[0138] This comparative example is used to compare and illustrate the thermal environment barrier coating and its preparation method disclosed in the present invention. The preparation method is the implementation steps of Example 3 except for the preparation part of the high entropy ceramic layer, that is, S1 to S4 in Example 3, and specifically includes the following steps:
[0139] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0140] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 500 mm, a spraying temperature of 650-800 °C, a spray gun speed of 500 mm / s, a spraying current of 1600 A, argon gas of 115 NLPM (standard liters per minute), and hydrogen gas of 5 NLPM;
[0141] S3. Preparation of Yb 2 Si 2 O 7 layer, the spraying distance is 900mm, the spraying temperature is controlled at 900-1100℃, the spraying gun travel is 700mm / s, the spraying current is controlled at 2550A, the argon flow rate is 95NLPM, and the helium flow rate is 30NLPM;
[0142] S4. After spraying Yb 2 Si 2 O 7 After coating, the sample was taken out and kept at 1300°C in air atmosphere for 3 hours with a heating and cooling rate of 5°C / min to obtain the target thermal environment barrier coating.
[0143] Performance Testing
[0144] The thermal environment barrier coatings prepared in Example 3 and Comparative Example 3 were subjected to water-oxygen corrosion tests in a 1400°C water-oxygen environment. The experimental conditions were: atmospheric atmosphere, a 1700X tube furnace was used to control the sample temperature to 1400°C ± 2°C, a 1600°C thermocouple was used to measure the temperature and feedback to adjust the tube furnace setting temperature, a water vapor flow rate of 23.2 g / min, introduced from one side of the tube furnace, and the other side of the tube furnace was connected to the atmosphere, and the water-oxygen corrosion time was 150 h. After water-oxygen corrosion, cross-section observation was performed, and the test results obtained were as follows: Figure 5 and Figure 6 As shown, the test remaining Yb 2 Si 2 O 7 The layer thickness and the Si layer thermally grown oxide thickness, the test results are filled in Table 3.
[0145] Table 3
[0146]
[0147] Depend on Figure 5 , Figure 6 As can be seen from the test results in Table 3, the Yb 2 Si 2 O 7 The surface of the layer was obviously corroded, and the surface flatness decreased; in Example 3, Yb 2 Si 2 O 7 The remaining thickness of the layer is significantly higher than that of the comparative example 3, and the thickness of the thermally grown oxide of the Si layer in the embodiment 3 is significantly lower than that of the comparative example 3, indicating that the high entropy ceramic layer with feather columnar structure can effectively 2 Si 2 O 7 The protective effect of the layer reduces the Yb 2 Si 2 O7 Corrosion of Si layer and Si layer in high temperature water and oxygen environment.
[0148] Example 4
[0149] This embodiment is used to illustrate the thermal environment barrier coating and the preparation method thereof disclosed in the present invention, including the following steps:
[0150] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0151] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 470 mm, a spraying temperature of 650-800 ° C, a spray gun speed of 470 mm / s, a spraying current of 1650 A, argon gas of 100 NLPM (standard liters per minute), and hydrogen gas of 5 NLPM;
[0152] S3. Preparation of Yb 2 Si 2 O 7 layer, the spraying distance is 1000mm, the spraying temperature is controlled at 900-1000℃, the spraying gun travel is 700mm / s, the spraying current is controlled at 2400A, the argon flow rate is 95NLPM, and the helium flow rate is 30NLPM;
[0153] S4. After spraying Yb 2 Si 2 O 7 After the layer, the sample was taken out and kept in an air atmosphere at 1300 °C for 3 hours with a heating and cooling rate of 5 °C / min;
[0154] S5. Prepared by PS-PVD technology (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 ) 2 Zr 2 O 7 For the high entropy ceramic layer, the spraying distance is controlled at 950mm, the spraying temperature is controlled at 900-1100℃, the spraying speed is 450mm / s, the current is controlled at 2550A, the argon flow rate is 40NLPM, and the helium flow rate is 70NLPM to obtain the target thermal environment barrier coating.
[0155] Comparative Example 4
[0156] This comparative example is used to compare and illustrate the thermal environment barrier coating and its preparation method disclosed in the present invention. The preparation method is the implementation steps of Example 4 except for the preparation part of the high entropy ceramic layer, that is, S1 to S4 in Example 4, and specifically includes the following steps:
[0157] S1. Use 60# sand to perform sand blasting at 0.6MPa, then use 120# corundum sand to perform sand blasting at 0.4MPa, and use anhydrous ethanol ultrasonic cleaning for 10min;
[0158] S2. The Si layer was prepared by PS-PVD technology, with a spraying distance of 470 mm, a spraying temperature of 650-800 ° C, a spray gun speed of 470 mm / s, a spraying current of 1650 A, argon gas of 100 NLPM (standard liters per minute), and hydrogen gas of 5 NLPM;
[0159] S3. Preparation of Yb 2 Si 2 O 7 layer, the spraying distance is 1000mm, the spraying temperature is controlled at 900-1000℃, the spraying gun travel is 700mm / s, the spraying current is controlled at 2400A, the argon flow rate is 95NLPM, and the helium flow rate is 30NLPM;
[0160] S4. After spraying Yb 2 Si 2 O 7 After coating, the sample was taken out and kept at 1300°C in air atmosphere for 3 hours with a heating and cooling rate of 5°C / min to obtain the target thermal environment barrier coating.
[0161] Performance Testing
[0162] 1. The thermal environment barrier coatings prepared in Example 4 and Comparative Example 4 were subjected to water-oxygen corrosion tests in a 1400°C water-oxygen environment. The experimental conditions were: atmospheric atmosphere, a 1700X tube furnace was used to control the sample temperature to 1400°C ± 2°C, a 1600°C thermocouple was used to measure the temperature and feedback was used to adjust the tube furnace setting temperature, the water vapor flow rate was 23.2 g / min, and it was introduced from one side of the tube furnace, and the other side of the tube furnace was connected to the atmosphere. The water-oxygen corrosion time was: 300h. After water-oxygen corrosion, the cross-section was observed, and the test results obtained were as follows: Figure 7 and Figure 8 As shown, the test remaining Yb 2 Si 2 O 7 The layer thickness and the Si layer thermally grown oxide thickness, the test results are filled in Table 4.
[0163] Table 4
[0164]
[0165] Depend on Figure 7 , Figure 8 As can be seen from the test results in Table 4, the Yb 2 Si2 O 7 The surface of the layer was obviously corroded, and the surface flatness decreased; in Example 4, Yb 2 Si 2 O 7 The remaining thickness of the layer is significantly higher than that of the comparative example 4, and the thickness of the thermally grown oxide of the Si layer in the embodiment 4 is significantly lower than that of the comparative example 4, indicating that the high entropy ceramic layer with feather columnar structure can effectively 2 Si 2 O 7 The protective effect of the layer reduces the Yb 2 Si 2 O 7 Corrosion of Si layer and Si layer in high temperature water and oxygen environment.
[0166] 2. The thickness of the thermally grown oxide of the Si layer obtained by the above Examples 2 to 4 and Comparative Examples 2 to 4 is plotted to obtain the following results: Figure 8 As shown, TEBC is the test results of Examples 2 to 4, and EBC is the test results of Comparative Examples 2 to 4.
[0167] Depend on Figure 8 It can be seen from the test results that the thermal environment barrier coating provided by the present invention has a good high-temperature water and oxygen barrier effect, effectively delays the growth of thermally grown oxides in the Si layer, and is beneficial to improving the service life of SiC components in a high-temperature water and oxygen environment.
[0168] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A thermal barrier coating, characterized in that: The invention comprises a dense layer and a high strain tolerance layer, wherein the dense layer comprises rare earth silicate, and the high strain tolerance layer comprises high entropy ceramic.
2. The thermal environment barrier coating according to claim 1, characterized in that: The high strain tolerance layer includes a plurality of feather column structures arranged on the surface of the dense layer, and the feather column structures are composed of the high entropy ceramic.
3. The thermal environment barrier coating according to claim 1, characterized in that: The high entropy ceramic comprises (Y 0.2 La 0.2 Nd 0.2 Sm 0.2 Eu 0.2 )2Zr2O7, and / or The rare earth silicate includes one or more of rare earth monosilicates and rare earth disilicates, and the rare earth elements of the rare earth silicate include one or more of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, yttrium and erbium.
4. The thermal environment barrier coating according to claim 1 or 3, characterized in that: The rare earth silicate is selected from rare earth double silicate, and the rare earth double silicate includes Yb2Si2O7.
5. The thermal environment barrier coating according to claim 1, characterized in that: The thickness of the dense layer is 75 to 200 μm, and / or The thickness of the high strain tolerance layer is 150-300 μm.
6. The thermal environment barrier coating according to claim 1, characterized in that: The invention also comprises a Si layer, wherein the Si layer is used for contacting with the substrate, the Si layer is located on a side of the dense layer away from the high strain tolerance layer, and the thickness of the Si layer is 50-150 μm.
7. A high temperature resistant component, characterized in that: The invention comprises a substrate and a thermal environment barrier coating according to any one of claims 1 to 6 arranged on the substrate, wherein the substrate is selected from SiC.
8. The method for preparing a thermal barrier coating according to any one of claims 1 to 6, characterized in that: The steps are as follows: Using rare earth silicates as raw materials, the dense layer is deposited; A high entropy ceramic is deposited on the surface of the dense layer to form a high strain tolerance layer.
9. The method for preparing a thermal environment barrier coating according to claim 8, characterized in that: Also includes: SiC is used as a substrate, a Si layer is deposited on the substrate, and the dense layer is formed on the Si layer.
10. The method for preparing a thermal environment barrier coating according to claim 9, characterized in that: The Si layer, the dense layer and the high strain tolerance layer are all prepared by PS-PVD technology; The PS-PVD preparation parameters of the Si layer are: spraying current of 1500-1700A, argon flow rate of 100-120 NLPM (standard liters per minute), hydrogen flow rate of 4-7 NLPM (standard liters per minute), and chamber pressure of 35-50 mbar; and / or The PS-PVD preparation parameters of the dense layer are: spraying current of 2400-2600A, argon flow rate of 90-110 NLPM (standard liters per minute), helium flow rate of 15-30 NLPM (standard liters per minute), and chamber pressure of 1.2-2.0 mbar; and / or The PS-PVD preparation parameters of the high strain tolerance layer are: the current is controlled at 2400-2600A, the argon flow rate is 25-45 NLPM (standard liters per minute), and the helium flow rate is 50-70 NLPM (standard liters per minute); and / or After the dense layer is sprayed, the sprayed dense layer is heat treated at a temperature of 1250 to 1350° C. for a time of 2 to 10 hours.
Citation Information
Patent Citations
Ultra-temperature thermal barrier coating and preparation method and application thereof and aeroengine
CN109295409A
Thermal-environmental barrier coating and preparation method and application thereof
CN113278909A
Self-healing high-density environmental barrier coating as well as preparation method and application thereof
CN114276169A
Thermal barrier coating as well as preparation method and application thereof
CN115011905A
High-entropy ceramic thermal barrier coating and preparation method thereof
CN116377372A
Cited By
Anti-corrosion and radar-infrared compatible stealth function integrated coating and preparation method thereof
CN121204592A