Grinding disc for efficiently grinding silicon carbide and preparation method of grinding disc

By using grinding sheets prepared by using melamine resin and diamond, a polymer mesh structure is formed through hot pressing process, the problems of short life and high cost of existing silicon carbide grinding tools are solved, and uniform and efficient grinding of silicon carbide materials is achieved Improved smoothness.

CN119036324APending Publication Date: 2024-11-29KAGES WINTER MASCH EQUIP (DALIAN) CO LTD

Patent Information

Application Number
CN202411374382.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing silicon carbide grinding tools have short lifespan and high cost, which cannot meet the needs of efficient grinding.

Method used

The grinding sheet is prepared using melamine resin, diamond, white corundum, silicon carbide, iron powder, calcium silicate and copper powder, and a polymer mesh structure is formed through hot pressing process to evenly wrap the diamond powder to improve the grinding sheet performance.

Benefits of technology

It achieves uniform and efficient grinding of silicon carbide materials, extends the life of the grinding sheet, reduces production costs, and improves flatness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036324A_ABST
    Figure CN119036324A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of silicon carbide high-hardness material grinding, in particular to a grinding disc for efficiently grinding silicon carbide and a preparation method of the grinding disc. Firstly, thermosetting melamine resin powder, diamond powder, copper powder, silicon carbide, iron powder and white corundum are sequentially put into a mixer to be stirred and mixed; the preparation method comprises the following steps: uniformly mixing and stirring the raw materials in a mixer, putting uniformly mixed solid powder into a mold, uniformly pressing the mixed material by using a flattening pair, then putting the mold for grinding the material into a hot press, fully curing and molding, and demolding the abrasive disc by using a demolding jig after curing is completed. According to the invention, the self-curing mechanism of the melamine resin is utilized, various grinding materials are uniformly mixed, and the melamine resin is subjected to a cross-linking reaction under the conditions of heating and pressurizing to form a high-molecular net structure, so that the silicon carbide slag on the silicon carbide grid can be ground, and the silicon carbide slag on the silicon carbide grid can be ground. The grinding material and the inorganic filler are wrapped to form the diamond grinding disc with stable performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding silicon carbide high-hardness materials, and in particular to a grinding disc for efficiently grinding silicon carbide and a preparation method thereof. Background Art

[0002] Abrasive discs are tools used for grinding. They fix abrasives in various ways to perform surface treatment on various materials. Abrasive discs have a wide range of applications, including but not limited to stone processing, metal material processing, pulp fiber processing, etc. According to different application scenarios and processing requirements.

[0003] For example, a diamond composite louver-blade abrasive tool as mentioned in CN219337423U comprises a substrate and a Velcro cloth provided on the back of the substrate, a plurality of diamond blocks 1 and silicon carbide blocks are provided on the front and circumferential direction of the substrate, the diamond blocks 1 and silicon carbide blocks are arranged at intervals and staggered, the diamond blocks 1 and silicon carbide blocks form a ring, a plurality of diamond blocks 2 are provided in the middle of the front of the substrate, the diamond blocks 2 are arranged at intervals along the circumference of the substrate to form a circular ring, a plurality of heat dissipation holes are provided on the circumferential outer side of the substrate, sound-absorbing cotton is provided in the intervals between the diamond block 1 and the silicon carbide block and in the intervals between the diamond block 2, the diamond block 1, the silicon carbide block and the diamond block 2 are arranged with equal height / equal thickness, and the sound-absorbing cotton is fixed on the substrate; a bevel is provided on the circumferential outer side of the diamond block, and the bevel is inclined toward the center of the substrate.

[0004] Most of the blades used for grinding silicon carbide materials on the market are louver blades, which are expensive and have a short grinding life. In order to increase the life and reduce the cost, a grinding disc for grinding silicon carbide and a preparation method thereof are proposed. Summary of the invention

[0005] The object of the present invention is to provide a grinding disc for efficiently grinding silicon carbide and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0006] To achieve the above object, one of the objects of the present invention is to provide a grinding sheet for efficiently grinding silicon carbide, comprising the following raw materials in parts by weight:

[0007] 20-28 parts by weight of melamine resin, 8-16 parts by weight of diamond, 8-16 parts by weight of white corundum, 20-30 parts by weight of silicon carbide, 10-18 parts by weight of iron powder, 5-9 parts by weight of calcium silicate, and 4-8 parts by weight of copper powder.

[0008] As a further improvement of the technical solution, the melamine resin is melamine molding compound powder.

[0009] As a further improvement of the technical solution, the diamond is 30 mesh diamond particles, the white corundum is 600 mesh white corundum, and the silicon carbide is 50 mesh silicon carbide.

[0010] The second object of the present invention is to provide a method for preparing the above-mentioned grinding disc for uniform grinding of silicon carbide, comprising the following steps:

[0011] S1. First, melamine resin and diamond are mixed to form a main material, and then the main material is put into a mixer for standby use;

[0012] S2, adding white corundum, silicon carbide, iron powder, calcium silicate powder and copper powder together and mixing them evenly;

[0013] S3, after fully mixing the above raw materials in a mixer, weigh a certain amount of powder, add it to a mold, flatten and compact it;

[0014] S4. Put the mold with abrasive into a hot press to heat and pressurize it so that the resin powder and various powders are fully solidified, and then use a demoulding machine to demould and take out the abrasive.

[0015] As a further improvement of the technical solution, in S1, 20-28 parts by weight of melamine resin powder and 10-14 parts by weight of diamond are firstly mixed uniformly.

[0016] As a further improvement of the present technical solution, in S2, 8-16 parts by weight of white corundum, 20-30 parts by weight of silicon carbide, 10-18 parts by weight of iron powder, 5-9 parts by weight of calcium silicate powder, and 4-8 parts by weight of copper powder are mixed and shaken evenly, and then added together and mixed evenly.

[0017] As a further improvement of the technical solution, in S3, when the mold temperature is 90-110° C., the above raw materials are fully mixed in a mixer, and then a certain mass of powder is weighed and added to the mold for flattening and compacting.

[0018] As a further improvement of the present technical solution, in S4, the mold with the abrasive is placed in a hot press and heated and pressurized to fully solidify the resin powder and various powders, and then the mold is demolded and the abrasive is taken out by a demolding machine, and the temperature range of the hot press is 150-180°C, and the pressure range of the hot press is 200-500Mpa.

[0019] In the present invention, step S1 is to preliminarily mix the resin powder with the smallest density and the diamond powder with the largest density, steps S2 and S3 are to mix other materials and the material in step S1 evenly to form an abrasive with stable performance, and step S4 is to convert the evenly mixed abrasive into a grinding disc and abrasive tool.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] In the grinding disc for efficiently grinding silicon carbide and the preparation method thereof, resin powder with the smallest density and diamond powder with the largest density are preliminarily mixed evenly, and then mixed evenly with other materials. The melamine resin will self-solidify under heating and pressure to form a polymer network structure, and the inorganic filler and diamond powder added subsequently will be evenly wrapped to form a diamond grinding disc with stable performance. Finally, the grinding disc produced can evenly and efficiently grind the silicon carbide material and make it have good flatness. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the accompanying drawings in the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The grinding disc is a kind of grinding disc made by heating solid resin powder and diamond material under specific pressure. The existing louver blades have low cost performance when grinding traditional silicon carbide materials and can only be dry-ground, which cannot meet customers' needs for water grinding.

[0025] One of the purposes of the present invention is to provide a grinding sheet for uniformly grinding silicon carbide, comprising the following raw materials in parts by weight:

[0026] 20-28 parts by weight of melamine resin powder, 8-16 parts by weight of diamond, 8-16 parts by weight of white corundum, 20-30 parts by weight of silicon carbide, 10-18 parts by weight of iron powder, 5-9 parts by weight of calcium silicate, and 4-8 parts by weight of copper powder.

[0027] Furthermore, the melamine resin powder is a melamine molding compound powder that can be heated and self-cured. This resin powder will undergo a self-curing reaction under heating and pressure to form a polymer network structure to uniformly wrap the inorganic filler and diamond powder added subsequently to form a diamond grinding disc with stable performance;

[0028] Furthermore, the diamond is 30 mesh diamond particles, the white corundum is 600 mesh white corundum, and the silicon carbide is 50 mesh silicon carbide. The 30 mesh single crystal diamond can form stable and efficient scratches on the surface of silicon carbide when grinding, which solves the problem that ordinary grinding discs cannot grind silicon carbide.

[0029] See also Figure 1As shown, the second object of the present invention is to provide a method for preparing the grinding disc for uniform grinding of silicon carbide as described above, and the specific steps are as follows:

[0030] S1. First, melamine resin powder and diamond are mixed evenly to form a main material, and then the main material is put into a mixer for standby use;

[0031] S2, mix the white corundum, silicon carbide, iron powder, calcium silicate powder and copper powder, shake them evenly, then add them together and mix them evenly;

[0032] S3, after fully mixing the above raw materials in a mixer at 20°C, weigh a certain amount of powder, add it to a mold, flatten and compact it, and keep the mold temperature at 90-110°C;

[0033] S4. Put the mold with abrasive into a hot press and heat and pressurize it to fully solidify the resin powder and various powders, then use a demoulding machine to demould and take out the abrasive. The temperature range of the hot press is 150-180℃, and the pressure range of the hot press is 400-800Mpa.

[0034] In the present invention, the resin powder with the smallest density and the diamond powder with the largest density are preliminarily mixed evenly, and then mixed evenly with other materials. The melamine resin will self-solidify under heating and pressure to form a polymer network structure, and the inorganic filler and diamond powder added subsequently will be evenly wrapped to form a diamond grinding disc with stable performance. Finally, the grinding disc produced can evenly and efficiently grind the silicon carbide material and make it have better flatness.

[0035] According to the differences in raw material dosage and process parameters during the manufacturing process, the grinding disc for efficiently grinding silicon carbide provided by the present invention is further described through the following specific embodiments.

[0036] Example 1

[0037] S1, first 20 weight parts of melamine resin powder and 14 weight parts of diamond are mixed uniformly to form a main material, and the main material is put into a mixer and reserved for standby;

[0038] S2, then 8 parts by weight of white corundum, 30 parts by weight of silicon carbide, 18 parts by weight of iron powder, 5 parts by weight of calcium silicate powder, and 5 parts by weight of copper powder are mixed and shaken evenly, and then added together and mixed evenly;

[0039] S3, after fully mixing the above raw materials in a mixer at 20°C, weigh a certain amount of powder, add it to a mold, flatten and compact it, and keep the mold temperature at 90°C;

[0040] S4. Put the mold with abrasive into a hot press and heat and pressurize it to fully solidify the resin powder and various powders, then use a demoulding machine to demould and take out the abrasive. The temperature range of the hot press is 150°C, and the pressure range of the hot press is 400Mpa.

[0041] Example 2

[0042] S1, first 24 weight parts of melamine resin powder and 12 weight parts of diamond are mixed uniformly to form a main material, and the main material is put into a mixer and reserved for standby;

[0043] S2, then 12 parts by weight of white corundum, 25 parts by weight of silicon carbide, 14 parts by weight of iron powder, 7 parts by weight of calcium silicate powder, and 6 parts by weight of copper powder are mixed and shaken evenly, and then added together and mixed evenly;

[0044] S3, after fully mixing the above raw materials in a mixer at 20°C, weigh a certain amount of powder, add it to a mold, flatten and compact it, and keep the mold temperature at 100°C;

[0045] S4. Put the mold with abrasive into a hot press and heat and pressurize it to fully solidify the resin powder and various powders, then use a demoulding machine to demould and take out the abrasive. The temperature range of the hot press is 160°C, and the pressure range of the hot press is 600Mpa.

[0046] Example 3

[0047] S1, first 28 parts by weight of melamine resin powder and 10 parts by weight of diamond are mixed evenly to form a main material, and the main material is put into a mixer and reserved for standby;

[0048] S2, then 16 parts by weight of white corundum, 20 parts by weight of silicon carbide, 10 parts by weight of iron powder, 8 parts by weight of calcium silicate powder, and 8 parts by weight of copper powder are mixed and shaken evenly, and then added together and mixed evenly;

[0049] S3, after fully mixing the above raw materials in a mixer at 20°C, weigh a certain amount of powder, add it to a mold, flatten and compact it, and keep the mold temperature at 110°C;

[0050] S4. Put the mold with abrasive into a hot press and heat and pressurize it to fully solidify the resin powder and various powders, then use a demoulding machine to demould and take out the abrasive. The temperature range of the hot press is 170°C, and the pressure range of the hot press is 800Mpa.

[0051] Table 1 Comparison of raw material dosage in Examples 1-3

[0052]

[0053] Table 2 Comparison of process parameters in Examples 1-3

[0054]

[0055]

[0056] Comparative Example 1

[0057] This comparative example is based on Example 1, except that the weight portion of melamine resin powder is set to 15 parts, and the rest remains unchanged. The specific steps are similar to those of Example 1, and will not be described in detail in this comparative example.

[0058] Comparative Example 2

[0059] This comparative example is based on Example 1, except that the weight proportion of melamine resin powder is set to 32 parts, and the rest remain unchanged. The specific steps are similar to those of Example 1, and will not be described in detail in this comparative example.

[0060] Comparative Example 3

[0061] This comparative example is based on Example 2, except that the weight of diamond is set to 8 parts, and the rest remains unchanged. The specific steps are similar to those of Example 2, and will not be repeated in this comparative example.

[0062] Comparative Example 4

[0063] This comparative example is based on Example 2, except that the weight of diamond is set to 20 parts, and the rest remains unchanged. The specific steps are similar to those of Example 2, and will not be repeated in this comparative example.

[0064] Comparative Example 5

[0065] This comparative example is based on Example 3, except that the mold temperature is set to 80° C., and the rest remain unchanged. The specific steps are similar to those of Example 3, and will not be repeated in this comparative example.

[0066] Comparative Example 6

[0067] In this comparative example, based on Example 3, the temperature of the hot press is set to 200° C., the pressure of the hot press is set to 700 MPa, and the rest remains unchanged. The specific steps are similar to those in Example 3, and will not be repeated in this comparative example.

[0068] Table 3 Comparison of raw material dosage in comparative examples 1-6

[0069]

[0070]

[0071] Table 4 Comparison of process parameters in comparative examples 1-6

[0072] Mold temperature / ℃ Heat press temperature / ℃ Hot press pressure / MPa Comparative Example 1 90 150 400 Comparative Example 2 90 150 400 Comparative Example 3 100 160 600 Comparative Example 4 100 160 600 Comparative Example 5 80 170 800 Comparative Example 6 110 200 700

[0073] Test example

[0074] Abrasive sheets were prepared according to the preparation methods provided in Examples 1-3 and Comparative Examples 1-6, respectively, and the grinding performance of the abrasive sheets was tested. The abrasive sheets were used to grind silicon carbide mesh covers (the mesh cover size was 25 cm*25 cm), and the average value of the number of silicon carbide mesh covers that could be grinded by the abrasive sheets was measured, and the measured values ​​were recorded in Table 5.

[0075] Table 5 Comparison of grinding performance of grinding discs of Examples 1-3 and Comparative Examples 1-6

[0076]

[0077]

[0078] According to Table 5, it can be seen that compared with Examples 1-6, the average number of grindable silicon carbide mesh covers of the grinding discs prepared in Examples 1-3 is greater than the average number of grindable silicon carbide mesh covers of the grinding discs prepared in the Comparative Examples, and the average number of grindable silicon carbide mesh covers of the grinding discs prepared in Examples is greater than 4.5, while the average number of grindable silicon carbide mesh covers of the grinding discs prepared in the Comparative Examples with different raw material amounts and process parameters is reduced. Therefore, under the working conditions of this embodiment, the average number of grindable silicon carbide mesh covers of the prepared grinding discs is higher, and the grinding performance of the grinding discs is better.

[0079] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a grinding disc for efficiently grinding silicon carbide, characterized in that: The following steps are involved: S1, first 20-28 parts by weight of melamine resin powder and 10-14 parts by weight of diamond are mixed evenly to form a main material, and the main material is put into a mixer and reserved for standby; S2, then add 8-16 parts by weight of white corundum, 20-30 parts by weight of silicon carbide, 10-18 parts by weight of iron powder, 5-9 parts by weight of calcium silicate powder, and 4-8 parts by weight of copper powder and mix them evenly; S3, after fully mixing the above raw materials in a mixer, weigh out the powder and add it to a mold to flatten and compact; S4. Put the mold with abrasive into a hot press to heat and pressurize it so that the resin powder and various powders are fully solidified, and then use a demoulding machine to demould and take out the abrasive.

2. The method for preparing a grinding disc for efficiently grinding silicon carbide according to claim 1, characterized in that: In S1, the melamine resin powder is melamine molding compound powder, and the diamond is 30 mesh diamond particles.

3. The method for preparing a grinding disc for efficiently grinding silicon carbide according to claim 1, characterized in that: In the S2, white corundum, silicon carbide, iron powder, calcium silicate and copper powder are mixed and shaken evenly.

4. The method for preparing a grinding disc for efficiently grinding silicon carbide according to claim 1, characterized in that: In S2, the white corundum is 600 mesh white corundum, and the silicon carbide is 50 mesh silicon carbide.

5. The method for preparing a grinding disc for efficiently grinding silicon carbide according to claim 1, characterized in that: In S3, when the mold temperature is 90-110° C., the uniformly mixed material is evenly flattened using a flattening tool.

6. The method for preparing a grinding disc for efficiently grinding silicon carbide according to claim 1, characterized in that: In S4, the temperature range of the hot press is 150-180° C., and the pressure range of the hot press is 400-800 MPa.

7. A grinding disc for efficiently grinding silicon carbide prepared according to the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Resin anchoring agent diamond grinding wheel and production method thereof

    CN101386154A

  • Polished crystal tile abrasive disc and preparation method thereof

    CN105563357A

  • Diamond grinding material grinding tool

    CN106799685A

  • Diamond grinding piece and preparation method thereof

    CN108296995A

  • Diamond resin binder abrasive disc and preparation method and application thereof

    CN110842800A

Cited By

  • High-hardness diamond polishing grinding block and preparation method thereof

    CN121403265A