Metal ion implanted lithium-manganese-rich positive electrode material as well as preparation method and application thereof
Through metal ion implantation technology, specific metal cations are injected into lithium-rich manganese positive electrode materials to form stable chemical bonds and surface coatings, solving the problems of material cycle stability and voltage capacity attenuation, and achieving efficient battery performance improvement and simplification Preparation process.
Patent Information
- Application Number
- CN202410988463.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-29
AI Technical Summary
The existing lithium-rich manganese positive electrode materials have poor cycle stability, fast voltage and capacity decay rates, and are unstable in chemical properties and expensive, making it difficult to meet the needs of commercial applications.
Using metal ion implantation technology, lithium-rich manganese positive electrode material is prepared through high-temperature spray drying and high-temperature sintering technology, and metal cations such as Al, Ce, Er, La, Nb are implanted into the metal ion implanter to adjust the implantation time and voltage to form More stable M-O chemical bonds and surface coatings improve material structural stability.
The cycle stability of lithium-rich manganese positive electrode material and the battery's long cycle performance are significantly improved, the voltage and capacity attenuation problems are reduced, the preparation process is simplified, and the first-circle capacity and cycle retention rate of the battery are improved.
Smart Images

Figure CN119038625A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium-ion batteries, and in particular relates to a metal ion-implanted lithium-manganese-rich positive electrode material, a preparation method and an application thereof. Background Art
[0002] With the crisis of non-renewable energy and the increasing pollution of ecological environment, the development of new clean energy storage devices has received widespread attention. Electrochemical energy storage and conversion equipment is one of the effective means to alleviate the environmental pollution and global warming problems caused by traditional energy sources such as coal and fossil fuels. Lithium-ion batteries (LI B) occupy an important position in the rechargeable battery market due to their large specific capacity, high voltage, high power, high efficiency and low environmental pollution, and are considered to be one of the most promising new generation energy storage technologies in this century. High-performance LI B can meet the needs of communications, portable electronic devices, electric vehicles and hybrid vehicles.
[0003] LIB is composed of positive electrode, negative electrode, electrolyte and separator, and its electrochemical performance depends largely on the active materials of the electrodes. The positive electrode material plays an important role in determining the performance of LIB. It is the main lithium ion (Li+) donor in the system, determines the capacity of LIB, and affects the cost of the battery. The general formula of lithium-rich manganese-based positive electrode materials is xLi2MnO3·(1-x)LiMO2, where M is a transition metal such as Ni, Co, and Mn. With the continuous improvement of battery power density requirements, the requirements for lithium battery capacity and cycle performance are also becoming higher and higher.
[0004] At present, the main methods for preparing lithium-rich manganese positive electrode materials are liquid phase coprecipitation, sol-gel, hydrothermal method, solid phase ball milling method, and spray pyrolysis method. The main means to improve electrochemical performance are surface coating, such as coating with materials such as aluminum oxide, aluminum fluoride, and lithium phosphate to reduce the grain boundary resistance of lithium ions and inhibit the release of lattice oxygen; secondly, doping, such as Cr and K+, can inhibit its voltage decay during the cycle and improve its cycle stability; thirdly, there is a hydrothermal synthesis method to obtain micron spheres formed by the agglomeration of layered nanocrystals, whose special morphology effectively improves the low-temperature cycle performance. Although the above methods have improved the performance of lithium-rich manganese positive electrode materials, there are still problems such as poor cycle stability, fast voltage and capacity decay rates, which do not meet commercial needs, and the modification methods are complicated to operate, inefficient, and have large losses.
[0005] The document with application number "201210429536.6" discloses "a method for preparing a positive electrode material of lithium manganese oxide battery doped with scandium by an ion implanter". First, a lithium source and a manganese source are mixed, and then scandium or scandium oxide is doped into the mixed powder by an ion implanter; the doped mixed powder is dissolved in water or an organic solvent for fine grinding, and the ground slurry is dried to form a precursor; the precursor is pretreated in an oxygen atmosphere, and then calcined at high temperature; after cooling, it is crushed and classified to obtain a finished product. Since the chemical properties of scandium itself are relatively unstable and expensive, it is very meaningful to develop a simple, efficient, low-cost, and environmentally friendly method to improve its electrochemical performance in all aspects to achieve the commercial application of high-energy-density layered lithium-rich manganese positive electrodes. Summary of the invention
[0006] The present invention provides a metal ion implanted lithium-rich manganese-based positive electrode material, a preparation method and an application thereof, which solve the problems of poor cycle stability, fast voltage and capacity decay rates, relatively unstable chemical properties and high prices of lithium-rich manganese-based positive electrode materials.
[0007] To achieve the above object, the present invention provides the following technical solution: a method for preparing a lithium-rich manganese-based positive electrode material by metal ion implantation, comprising the following steps:
[0008] Step 1: Weigh a lithium source, a nickel source, a cobalt source, a manganese source, and a complexing agent according to the molar percentage of the elements Li:Ni:Co:Mn=1.53:0.165:0.165:0.665 and dissolve them in water to obtain a uniformly mixed precursor solution;
[0009] Step 2: obtaining a precursor powder of the material by high temperature spray drying the precursor solution;
[0010] Step 3: sintering the above-mentioned precursor powder at high temperature to obtain lithium-rich manganese positive electrode powder material;
[0011] Step 4: Place the weighed lithium-manganese-rich cathode powder material into the cavity of the metal ion implanter, assemble the target metal target material, and turn on the mechanical pump and molecular pump to evacuate the cavity;
[0012] Step 5: Turn on the trigger control, set the trigger frequency to 2-8, set the voltage to 2000-7000V, turn on the gas high-pressure chamber power supply to preheat, turn on the valve control, cleaning, and air intake; purify the chamber, turn on the cathode control, and set the voltage to 20-100V;
[0013] Step 6: Turn on the high voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, and start ion implantation;
[0014] Step 7: After 0.5-8 hours, turn off the metal source, turn off the cathode control voltage, turn off the high-voltage chamber, turn off the air intake, turn off the trigger power supply and power on, turn off the molecular pump and mechanical pump, and perform cavity venting sampling to obtain a lithium-rich manganese-based positive electrode material injected with metal ions.
[0015] Furthermore, in the above step 1, the lithium source, nickel source, cobalt source, and manganese source are selected from one or a combination of sulfate, nitrate, acetate, and oxalate; the complexing agent is any one of citric acid, ammonia water, carbonate, and bicarbonate, and the solubility of the precursor solution is 0.1 to 10 mol / L; the solubility of the complexing agent in the precursor solution is 0.05 to 5 mol / L.
[0016] Furthermore, in the above step 2, the inlet temperature of the spray drying is 150-280°C, the outlet temperature is 70-120°C, the peristaltic pump speed is 200-1000ml / h, the needle passing frequency is 5-30Hz, and the spray pressure is 0.1-0.5MPa; the atmosphere of the spray drying is one or more atmospheres of air and oxygen.
[0017] Furthermore, the specific operation of high temperature sintering in the above step three is: feeding the precursor powder into a muffle furnace, heating the temperature from room temperature to 600°C to 1200°C at a heating rate of 1°C / min to 10°C / min, keeping the temperature for 0.2 to 24 hours, and then cooling naturally.
[0018] Furthermore, the target metal element connected in the above step 4 is beryllium (Be), boron (B), sodium (Na), magnesium (Mg), phosphorus (P), sulfur (S), aluminum (Al), potassium (K), calcium (Ca), cerium (Ce), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), erbium (Er), zinc (Zn), gallium (Ga), germanium (Ge), arsenic (As), rubidium (Rb), lanthanum (La), strontium (Sr), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), indium (I n), tin (Sn), antimony (Sb), tellurium (Te), titanium (Ti), cesium (Cs), barium (Ba) One or a combination of several of them.
[0019] Furthermore, the target metal element introduced in the above step 4 is preferably one or a combination of aluminum (Al), cerium (Ce), erbium (Er), lanthanum (La), niobium (Nb), and titanium (Ti).
[0020] Furthermore, in the above step 4, titanium (Ti) is preferred.
[0021] Furthermore, in step 4, the chamber is vacuumed to 1.5x10 -4 Pa.
[0022] The above preparation method obtains a metal ion-implanted lithium-rich manganese-based positive electrode material.
[0023] Furthermore, the application of the above-mentioned metal ion implantation lithium-rich manganese-based positive electrode material is to prepare the lithium-rich manganese-based positive electrode material into a lithium-rich manganese-based positive electrode sheet, the lithium-rich manganese-based positive electrode material, the conductive agent (SuperP) and the binder (sodium carboxymethyl cellulose CMC) are mixed into a slurry in a mass ratio of 85:10:5, and the slurry is coated on an aluminum foil current collector with a scraper to obtain a positive electrode sheet to prepare a button battery.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. In the dynamic cycle process of lithium-rich manganese positive electrode materials, redox reactions occur continuously, and the precipitation of lattice oxygen, immersion in electrolyte, and transmission of ions cause the layered structure of the material to collapse, and the material cycle performance is greatly reduced. The element ratio of the lithium-rich manganese-based positive electrode material provided by the present invention is more reasonable. On this basis, metal cations are injected into the lithium-rich manganese-based positive electrode material by ion implantation to achieve metal cation doping substitution, provide a stronger MO chemical bond than active transition metals such as Ni, Co, and Mn (M), and improve the structural stability of the material by inhibiting the precipitation of lattice oxygen under high voltage, thereby improving the cycle stability of the lithium-rich manganese-based positive electrode material.
[0026] 2. The present invention adopts a high-voltage ion implanter to inject Al, Ce, Er, La, Nb, Ti, etc. as material sources, adjusts the injection time to control the amount of metal ion doping, and non-destructively, quickly, and accurately implants the target ions into lithium-rich manganese with controllable content. At the same time, during the preparation process, specific process parameters are used to adjust the injection time and the amount of metal cation doping. By occupying atomic positions to improve the structural stability of the positive electrode material and forming a surface coating, uniform doping of metal elements is achieved, the battery cycle stability is improved, and the long cycle performance, voltage and capacity attenuation of lithium batteries are greatly improved.
[0027] 3. The preparation method of the present invention is simple and easy to operate. When processing the electrode material, by adjusting the mass percentage of the binder, the thickness of the prepared lithium-rich manganese positive electrode material sheet is made more uniform and less likely to peel off.
[0028] 4. The lithium-rich manganese-based positive electrode material of the present invention has a battery first-cycle capacity of more than 323 mAh / g at a voltage of 4.8 V, and a first-cycle efficiency of up to 81.81%. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The electrochemical first cycle charge and discharge curve data of Examples 1-6 and the comparative example.
[0030] Figure 2The electrochemical cycle discharge capacity curve data of Examples 1-6 and the comparative example.
[0031] Figure 3 The electrochemical cycle discharge median voltage curve data of Examples 1-6.
[0032] Figure 4 The following are scanning electron microscope images of Examples 1-6 and a comparative example.
[0033] Figure 5 The X-ray diffraction data of the standard lithium-rich manganese material prepared in comparative example.
[0034] Figure 6 This is a scanning electron microscope image of the standard lithium-rich manganese material prepared in comparative example. DETAILED DESCRIPTION
[0035] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0036] The present invention adopts lithium-manganese-rich positive electrode material with specific element composition, realizes doping substitution of metal cations through metal ion implantation technology, adjusts process parameters and implantation time, and realizes structural modification of the lithium-manganese-rich positive electrode material.
[0037] Example 1: A metal ion (Al 3+ The method for preparing a lithium-rich manganese-based positive electrode material by injecting cations therein comprises the following steps:
[0038] Step 1: Synthesize 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 uses lithium acetate, nickel acetate, cobalt acetate, and manganese acetate, which are dissolved in deionized water in a stoichiometric ratio of 1.2:0.13:0.13:0.54 to prepare a 2 mol / L mixed salt solution, and 3 mol / L of chelating agent citric acid is added to the solution, and the solution is stirred on a magnetic stirrer for 1 hour to mix the solution evenly.
[0039] Step 2: Pump the mixed spray solution into the spray dryer, select an inlet air temperature of 230°C, an outlet air temperature of 115°C, a peristaltic pump speed of 600-800 ml / h, a needle passing frequency of 15 Hz, and a spray pressure of 0.2 MPa.
[0040] Step 3: Collect the precursor after spraying, place it in a corundum boat, send it into a crucible and calcine it in a muffle furnace, the heating rate is 3℃ / min, and keep it warm for 20 minutes after reaching 1000℃, during which fresh air is continuously introduced into the muffle furnace. After cooling in the furnace, the lithium-rich manganese positive electrode powder material is obtained.
[0041] Step 5. Set the trigger frequency to 8, set the voltage to 2000V, turn on the gas high-pressure chamber power preheating, turn on valve control, cleaning, air intake, purify the cavity, turn on cathode control, and set the voltage to 20V.
[0042] Step 6: Turn on the high voltage power supply, set the current to 6 mA, set the voltage to 10 kV, and start ion implantation;
[0043] Step seven, after 2 hours, turn off the metal source, turn off the cathode control voltage, turn off the high-voltage chamber, turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain Al ion-implanted lithium-manganese-rich positive electrode material, recorded as (Al-LMR).
[0044] Example 2: The preparation process is the same as that of Example 1, except that the injected metal cation is Ti.
[0045] The preparation process is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 material is weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor is obtained after spray drying. The precursor is placed in an oxygen atmosphere, and the temperature is raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it is cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LMR) is weighed and placed in a high-pressure ion implantation chamber, and the target material Ti is assembled. The mechanical pump and molecular pump are turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the chamber, set the trigger frequency to 8, set the voltage to 2000V, turn on the cathode control, and set the voltage to 20V. Turn on the high-voltage power supply, set the current to 6mA, set the voltage to 10kV, set it to the target voltage, and start the ion implantation experiment. The metal implantation time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the chamber for sampling to obtain the Ti ion-implanted lithium-manganese-based positive electrode material, recorded as (Ti-LMR).
[0046] Example 3: The preparation process is the same as that of Example 1, except that the injected metal cation is Ce.
[0047] The preparation process is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 material is weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor is obtained after spray drying. The precursor is placed in an oxygen atmosphere, and the temperature is raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it is cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LMR) is weighed and placed in a high-pressure ion implantation chamber, and the target material Ce is assembled. The mechanical pump and molecular pump are turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the chamber, set the trigger frequency to 8, set the voltage to 2000V, turn on the cathode control, and set the voltage to 20V. Turn on the high-voltage power supply, set the current to 6mA, set the voltage to 10kV, set to the target voltage, and start the ion implantation experiment. The metal implantation time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the chamber for sampling to obtain the Ce ion-implanted lithium-rich manganese-based positive electrode material, recorded as (Ce-LMR).
[0048] Example 4: The preparation process is the same as that of Example 1, except that the injected metal cation is Er.
[0049] The preparation process is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 material is weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor is obtained after spray drying. The precursor is placed in an oxygen atmosphere, and the temperature is raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it is cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LNCM) is weighed and placed in a high-pressure ion implantation chamber, and the target Er is assembled. The mechanical pump and molecular pump are turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the chamber, set the trigger frequency to 8, set the voltage to 2000V, turn on the cathode control, and set the voltage to 20V. Turn on the high-voltage power supply, set the current to 6mA, set the voltage to 10kV, set to the target voltage, and start the ion implantation experiment. The metal implantation time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the chamber for sampling to obtain the Er ion-implanted lithium-rich manganese-based positive electrode material, recorded as (Er2-LMR).
[0050] Example 5: The preparation process is the same as that of Example 1, except that the injected metal cation is La.
[0051] The preparation process is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni0.33 Co 0.33 Mn 0.33 )O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LMR) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the chamber, set the trigger frequency to 8, set the voltage to 2000V, turn on the cathode control, and set the voltage to 20V. Turn on the high-voltage power supply, set the current to 6mA, set the voltage to 10kV, set it to the target voltage, and start the ion implantation experiment. The metal implantation time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the chamber for sampling to obtain the La ion-implanted lithium-manganese-based positive electrode material, recorded as (La-LMR).
[0052] Example 6: The preparation process is the same as that of Example 1, except that the injected metal cation is Nb.
[0053] The preparation process is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LMR) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the chamber, set the trigger frequency to 8, set the voltage to 2000V, turn on the cathode control, and set the voltage to 20V. Turn on the high-voltage power supply, set the current to 6mA, set the voltage to 10kV, set to the target voltage, and start the ion implantation experiment. The metal implantation time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the chamber for sampling to obtain the Nb ion-implanted lithium-rich manganese-based positive electrode material, recorded as (Nb-LMR).
[0054] Comparative Example: The preparation process is the same as Example 1, except that no metal cation injection is performed.
[0055] Select the basic 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 layered lithium-rich manganese-based positive electrode material was experimented, similar to Example 1, the temperature was increased from room temperature to 500°C at a rate of 5°C / min, and then the temperature was increased to 800°C at a rate of 5°C / min after being kept constant for 3 hours. After being kept constant for 10 hours, it was naturally cooled to room temperature. The stoichiometric ratio of lithium acetate: nickel acetate: cobalt acetate: manganese acetate was 1.2:0.13:0.13:0.54, and a 2 mol / L mixed metal salt solution was prepared. Granulation was performed by spray drying to prepare a precursor of the layered lithium-rich manganese-based positive electrode material.
[0056] The precursor was placed in a muffle furnace with air for sintering, and the temperature was increased from room temperature to 1000°C at a heating rate of 5°C / min and kept constant for 20 minutes, and then naturally cooled to room temperature.
[0057] Test analysis:
[0058] The lithium-rich manganese-based positive electrode material, conductive agent (SuperP), and binder (sodium carboxymethyl cellulose CMC) obtained in Examples 1-6 and the comparative example were mixed into a slurry in a mass ratio of 85:10:5. After stirring at a stirring rate of 500 rad / min and stirring evenly, a positive electrode sheet was obtained by coating it on an aluminum foil current collector with a scraper. The scraper thickness was 0.2 mm, the vacuum oven temperature was 110°C, and the time was 20 h to obtain a lithium-rich manganese-based positive electrode sheet.
[0059] The lithium-rich manganese-based positive electrode sheets were cut into round pieces of uniform size, dried, and assembled into 2025 button batteries in a glove box filled with argon gas with oxygen and water content less than 0.01ppm. The button batteries were placed in an oven for long-term activation treatment at a temperature of 45°C and a treatment time of 40h. After being taken out, the battery cycle performance test was carried out at different current densities.
[0060] The electrochemical performance was tested by charging and discharging 2025 button cells on the Xinwei test system.
[0061] Metal Li sheet was used as reference electrode and counter electrode, Celgard-2400 was used as diaphragm, Xinzhoubang 3045I was used as electrolyte, and the test voltage window was 2.0~4.8V. The test temperature was 27±1℃, and the first three cycles were activated at 0.1C rate (1C=200mAh / g), and 1C rate was used from the 4th cycle. The performance test results are shown in Table 1.
[0062] Table 1
[0063]
[0064]
[0065] As can be seen from Table 1, Examples 1-6 show that the first discharge capacity of the battery prepared by the metal ion implantation lithium-rich manganese-based positive electrode material of the present invention can reach up to 323.30 mAh / g, and the capacity retention rate after 100 cycles can reach up to 90.59% or more.
[0066] See also Figure 1 : From the comparison of Examples 1-6, it can be seen that in the process of preparing the lithium-rich manganese-based positive electrode material by metal ion injection of the present invention, under the same injection time conditions, the first-cycle charge and discharge capacity of the battery prepared by the metal Ti-injected lithium-rich manganese-based positive electrode material is higher than that of the other metal-injected lithium-rich manganese-based positive electrode material batteries, and the 100-cycle capacity retention rate of the battery prepared by the metal Er-injected lithium-rich manganese-based positive electrode material is higher than that of the other metals.
[0067] See also Figure 2 : It can be seen from the comparison between Examples 1 and 2 and the comparative example that the injection of metal Ti into the lithium-rich manganese-based positive electrode material of the present invention improves the structural stability of its lithium-rich layered oxide and enhances the first cycle capacity and capacity retention rate of the battery.
[0068] By comparing Examples 1-6 and the comparative example, it can be seen that when the Ti metal ion injection time is 2h, the first discharge capacity of the battery made of lithium-rich manganese-based positive electrode material reaches up to 323.30mAh / g, and it also has relatively high cycle stability, with a capacity retention rate of up to 83.18% after 100 cycles.
[0069] See also Figure 3 : It can be seen from the comparison between Examples 1-6 and the comparative example that the injection of lanthanide metal ions into the lithium-rich manganese-based positive electrode material of the present invention can effectively improve the structural stability and electrochemical performance of the lithium-rich layered oxide thereof.
[0070] See also Figure 4 and Figure 6 : From the comparison of the organizational morphology of Examples 1-6 and the comparative example, it can be seen that the particle size of the lithium-rich manganese positive electrode material implanted with Ti ions is relatively small and the distribution is more uniform, which is beneficial to the improvement of the battery capacity and cycle stability.
[0071] See also Figure 5 : The injection of Ti ions causes a small shift in the peak of the lithium-manganese-rich material, indicating that Ti metal ions have been injected into the material, increasing the lattice spacing and the structural stability.
[0072] In summary, embodiment 2 is the best embodiment.
[0073] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a lithium-rich manganese-based positive electrode material by metal ion implantation, It is characterized in that The following steps are involved: Step 1: Weigh a lithium source, a nickel source, a cobalt source, a manganese source, and a complexing agent according to the molar percentage of the elements Li:Ni:Co:Mn=1.53:0.165:0.165:0.665 and dissolve them in water to obtain a uniformly mixed precursor solution; Step 2: obtaining a precursor powder of the material by high temperature spray drying the precursor solution; Step 3: sintering the above-mentioned precursor powder at high temperature to obtain lithium-rich manganese positive electrode powder material; Step 4: Place the weighed lithium-manganese-rich cathode powder material into the cavity of the metal ion implanter, assemble the target metal target material, and turn on the mechanical pump and molecular pump to evacuate the cavity; Step 5: Turn on the trigger control, set the trigger frequency to 2-8, set the voltage to 2000-7000V, turn on the gas high-pressure chamber power supply to preheat, turn on the valve control, cleaning, and air intake; purify the chamber, turn on the cathode control, and set the voltage to 20-100V; Step 6: Turn on the high voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, and start ion implantation; Step 7: After 0.5-8 hours, turn off the metal source, turn off the cathode control voltage, turn off the high-voltage chamber, turn off the air intake, turn off the trigger power supply and power on, turn off the molecular pump and mechanical pump, and perform cavity venting sampling to obtain a lithium-rich manganese-based positive electrode material injected with metal ions.
2. The method for preparing a metal ion-implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that In the step 1, the lithium source, nickel source, cobalt source, and manganese source are selected from one or a combination of sulfate, nitrate, acetate, and oxalate; the complexing agent is any one of citric acid, ammonia water, carbonate, and bicarbonate, and the solubility of the precursor solution is 0.1~10mol / L; the solubility of the complexing agent in the precursor solution is 0.05~5mol / L.
3. The method for preparing a metal ion-implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that In the step 2, the inlet temperature of the spray drying is 150-280°C, the outlet temperature is 70-120°C, the peristaltic pump speed is 200-1000ml / h, the needle passing frequency is 5-30Hz, and the spray pressure is 0.1-0.5MPa; the atmosphere of the spray drying is one or more atmospheres of air and oxygen.
4. The method for preparing a metal ion-implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that The specific operation of high temperature sintering in step three is: feeding the precursor powder into a muffle furnace, heating the temperature from room temperature to 600°C~1200°C at a heating rate of 1°C / min~10°C / min, keeping the temperature for 0.2~24 hours, and then cooling naturally.
5. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that In the step 4, the target metal element connected is beryllium (Be), boron (B), sodium (Na), magnesium (Mg), phosphorus (P), sulfur (S), aluminum (Al), potassium (K), calcium (Ca), cerium (Ce), vanadium (V), chromium (Cr), iron (Fe), copper (Cu), erbium (Er), zinc (Zn), gallium (Ga), germanium (Ge), arsenic (As), rubidium (Rb), lanthanum (La), strontium (Sr), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), indium (In), tin (Sn), antimony (Sb), tellurium (Te), titanium (Ti), cesium (Cs), barium (Ba) One or a combination of several.
6. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that The target metal element introduced in step 4 is preferably one or a combination of aluminum (Al), cerium (Ce), erbium (Er), lanthanum (La), niobium (Nb), and titanium (Ti).
7. The method for preparing a metal ion-implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that In the step 4, titanium (Ti) is preferred.
8. The method for preparing a metal ion-implanted lithium-rich manganese-based positive electrode material according to claim 1, It is characterized in that In step 4, the chamber is vacuumed to 1.5x10 -4 Pa.
9. A metal ion-implanted lithium-rich manganese-based positive electrode material obtained by the preparation method according to claim 1.
10. Use of a metal ion-implanted lithium-rich manganese-based positive electrode material according to claim 8, It is characterized in that The lithium-rich manganese-based positive electrode material is prepared as a lithium-rich manganese-based positive electrode sheet. The lithium-rich manganese-based positive electrode material, a conductive agent (SuperP) and a binder (sodium carboxymethyl cellulose CMC) are mixed into a slurry at a mass ratio of 85:10:5, and the slurry is coated on an aluminum foil current collector by a scraper to obtain a positive electrode sheet, thereby preparing a button battery.
Citation Information
Cited By
Lithium-rich manganese-based positive electrode material with core-shell structure and preparation method of lithium-rich manganese-based positive electrode material
CN121726383A