Shield backfill grouting slurry and preparation method thereof

CN119038913APending Publication Date: 2024-11-29CHINA RAILWAY 14TH BUREAU GRP LARGE SHIELD ENG CO LTD +2
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202410803910.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing back-wall grouting slurry with contradictory injectable and curing strength. If the strength is high, the injectable is poor, and if the weak is weak, the curing is not firm, which affects the quality of the project.

Method used

Using a slurry formula including water, curing agent, silicate cement and silty clay, hemihydrate gypsum, calcium aluminate, silica fine powder, alumite and quicklime are added to the curing agent, and expandable ettringite is formed by stirring and mixing. Improve the strength and impermeability of the slurry, and use silty clay as a skeleton material to ensure infusion.

Benefits of technology

The high fluidity of the slurry during transportation and the instantaneous increase in strength after injection is achieved, while improving waterproofing performance and engineering quality, ensuring the stability and waterproofing ability of the shield tunnel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038913A_ABST
    Figure CN119038913A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of shield grouting, in particular to shield wall post-grouting slurry and a preparation method thereof.The shield wall post-grouting slurry comprises water and the following components in percentage by weight: 8-10% of a curing agent, 8-12% of Portland cement and 78-84% of silty clay, and the weight of the water is 90-95% of the total weight of the curing agent, the Portland cement and the silty clay. The raw materials of the shield wall post-grouting slurry are all fine powder, the groutability is ensured while the strength is ensured, and the silty clay plays a role of a framework and ensures the groutability of the slurry. According to the shield wall post-grouting slurry, the groutability in the transportation process is guaranteed, the high fluidity before grouting is guaranteed, the strength can be instantly increased after the slurry is injected, and meanwhile the problem that the quality of a wall post-grouting project is affected due to the fact that ordinary slurry is poor in waterproof performance in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shield grouting, and in particular to a shield wall back-grouting slurry and a preparation method thereof. Background Art

[0002] Shield construction refers to a construction method in which a tunnel with a diameter equivalent to the designed tunnel is excavated in the stratum, and the prefabricated tunnel lining is installed on the tunnel wall during the excavation process by a shield machine to form a stable tunnel structure.

[0003] The loss of strata caused by shield construction and the disturbance of soil around the shield tunnel are important reasons for the settlement of the ground surface and shield grouting materials. In order to reduce and prevent settlement, during the shield excavation process, a sufficient amount of slurry material should be injected behind the lining segment that has escaped from the shield tail as soon as possible to fill the shield tail annular shield grouting gap. Grouting slurry is the main material that plays a filling and consolidation role in the stratum cracks and pores. Its functions mainly include the following three aspects: 1. Fill the shield tail gap in time, support the rock mass around the segment, and effectively control the surface settlement. 2. The consolidated slurry will serve as the first waterproof barrier of the shield construction tunnel and enhance the waterproof ability of the tunnel. 3. The consolidated slurry integrates the segment with the surrounding rock mass, which is conducive to the control of the shield excavation direction and can ensure the final stability of the shield tunnel.

[0004] Existing grouting materials can be divided into granular slurry, chemical slurry and fine mineral slurry. Since the strength of ordinary slurry in the prior art is generally inversely proportional to the water content, while the viscosity of the slurry is proportional to the water content, the shield wall back-injection slurry on the market currently generally has a contradiction between injectability and solidification strength. Strong injectability means low strength, while high strength means poor injectability. Summary of the invention

[0005] In order to solve the technical problem that the shield wall back-grouting slurry currently on the market generally has a contradiction between injectability and solidification strength, that is, strong injectability leads to low strength, and high strength leads to poor injectability, the present invention provides a shield wall back-grouting slurry and a preparation method thereof.

[0006] To achieve the above purpose, a technical solution adopted by a shield wall back grouting slurry in the present invention is: A shield wall back-grouting slurry comprises water and the following components in weight percentage: 8-10% of a curing agent, 8-12% of silicate cement and 78-84% of silty clay, wherein the weight of water is 90%-95% of the total weight of the curing agent, silicate cement and silty clay.

[0007] By adopting the above scheme, the raw materials of the shield wall back injection slurry in the present invention are all fine powder, which ensures strength and injectability, wherein the silty clay plays a role of skeleton and ensures the injectability of the slurry. The shield wall back injection slurry in the present invention ensures injectability during transportation and high fluidity before grouting. The strength of the slurry can be instantly increased after injection, and the problem of poor waterproof performance of ordinary slurry in the prior art is solved, which affects the quality of the back injection grouting project.

[0008] As a preferred implementation method of the grouting slurry for the back injection of a shield wall, the weight percentages of the curing agent, silicate cement and silty clay are: 10% curing agent, 10% silicate cement and 80% silty clay.

[0009] As a preferred implementation method of the shield wall back-grouting slurry, the curing agent includes hemihydrate gypsum, calcium aluminate, silica powder, alunite and quicklime.

[0010] By adopting the above scheme, the alunite in the curing agent can quickly form expansive ettringite under the stimulation of hemihydrate gypsum, and the silicate cement reacts with hemihydrate gypsum and calcium aluminate to quickly form expansive ettringite, which can accelerate the solidification of the slurry and improve the strength and impermeability of the slurry consolidation body. The silicon micropowder in the curing agent can effectively improve the stability, temperature resistance, and acid and alkali corrosion resistance of the slurry consolidation body. The quicklime in the curing agent reacts with the silicon micropowder to improve the strength of the material.

[0011] As a preferred implementation method of grouting slurry for back injection of a shield wall, the weight percentages of hemihydrate gypsum, calcium aluminate, silica micropowder, alunite and quicklime in the curing agent are: 8-12% hemihydrate gypsum, 40-45% calcium aluminate, 30-40% silica micropowder, 5-10% alunite and 5-10% quicklime.

[0012] As a preferred implementation method of grouting slurry for back injection of a shield wall, the weight percentages of hemihydrate gypsum, calcium aluminate, silica powder, alunite and quicklime are: 10% hemihydrate gypsum, 40% calcium aluminate, 35% silica powder, 5% alunite and 10% quicklime.

[0013] As a preferred implementation of the shield wall back-grouting slurry, the weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0014] The technical solution adopted by the method for preparing a shield wall back-grouting slurry in the present invention is as follows: A method for preparing a shield wall back-grouting slurry is used to prepare any of the above-mentioned shield wall back-grouting slurry, comprising the following steps: adding water to the prepared curing agent, silicate cement and silty clay, and stirring and mixing.

[0015] By adopting the above scheme, the shield wall rear grouting slurry in the present invention can be prepared by adding water to the raw materials and mixing and stirring. The grouting slurry has strong injectability and can be used in ordinary grouting machines. The requirements for grouting equipment are relatively low, which greatly improves the practical range of the grouting slurry.

[0016] As a preferred implementation of a method for preparing a shield wall back-injection slurry, the preparation of a curing agent includes the following steps: placing hemihydrate gypsum, calcium aluminate, silica powder, alum stone, and quicklime in a mixing device, mixing and stirring for 3 to 5 minutes.

[0017] As a preferred implementation of a method for preparing a grouting slurry for back injection of a shield wall, the stirring speed for adding water and stirring and mixing is 600 to 700 r / min, and the stirring time is 8 to 10 min.

[0018] The beneficial effects of the present invention include: The raw materials of the shield wall back grouting slurry in the present invention are all fine powder, which ensures strength and injectability. The shield wall back grouting slurry in the present invention ensures injectability during transportation and high fluidity before grouting. The strength of the slurry can be instantly increased after injection, and the problem of poor waterproof performance of ordinary slurry is solved, which affects the quality of the back wall grouting project.

[0019] The shield wall back grouting slurry in the present invention can be prepared into a grouting slurry with high strength, strong waterproofness, strong temperature resistance, and strong acid and alkali corrosion resistance through the coordination of raw materials. Specifically, the alunite in the curing agent can quickly form expansive calcium sulfonite under the stimulation of semi-hydrated gypsum, and the silicate cement reacts with semi-hydrated gypsum and calcium aluminate to also quickly form expansive calcium sulfonite, which can accelerate the solidification of the slurry and improve the strength and impermeability of the slurry consolidation body. The silicon micropowder in the curing agent can effectively improve the stability, temperature resistance, and acid and alkali corrosion resistance of the slurry consolidation body. The quicklime in the curing agent reacts with the silicon micropowder to improve the strength of the material. The silty clay plays a skeleton role and ensures the injectability of the slurry.

[0020] The shield wall rear grouting slurry in the present invention can be prepared by adding water to raw materials, mixing and stirring. The grouting slurry has strong injectability and can be used in ordinary grouting machines. The requirements for grouting equipment are relatively low, which greatly improves the practical scope of the grouting slurry. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 This is a flow chart of a method for preparing a shield wall post-grouting slurry in Example 1. DETAILED DESCRIPTION

[0022] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical scheme of the present invention will be clearly and completely described below in conjunction with the drawings in this specific embodiment. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0023] Embodiment 1: Reference Figure 1 This embodiment provides a method for preparing a shield wall post-grouting slurry, comprising the following steps: S1. Place hemihydrate gypsum, calcium aluminate, silica powder, alum stone and quicklime in a mixing device, mix and stir for 3 to 5 minutes to prepare a curing agent; S2. Add water to the prepared curing agent, silicate cement and silty clay in proportion and stir them evenly. The stirring speed of adding water and stirring is 600-700r / min, and the stirring time is 8-10min. After the stirring is completed, the grouting slurry is obtained.

[0024] In this embodiment, the stirring time of hemihydrate gypsum, calcium aluminate, silica powder, alunite and quicklime can be 3 minutes, 4 minutes or 5 minutes.

[0025] In this embodiment, the stirring speed of adding water and stirring and mixing can be 600 r / min or 700 r / min, and the stirring time can be 8 min, 9 min or 10 min.

[0026] Embodiment 2: This embodiment provides a method for preparing a shield wall back-grouting slurry, comprising the following steps: S1, hemihydrate gypsum, calcium aluminate, silica powder, alum stone and quicklime are placed in a mixing device and mixed and stirred for 5 minutes to prepare a curing agent; S2. Add water to the prepared curing agent, silicate cement and silty clay in proportion and stir them evenly. The stirring speed of adding water and stirring is 700r / min, and the stirring time is 10min. After the stirring is completed, the grouting slurry is obtained.

[0027] Embodiment 3: This embodiment proposes a shield wall back grouting slurry, including water and the following weight percentages of components: 8-10% of curing agent, 8-12% of silicate cement and 78-84% of silty clay. The weight percentages of hemihydrate gypsum, calcium aluminate, silica powder, alum stone and quicklime in the curing agent are: 8-12% of hemihydrate gypsum, 40-45% of calcium aluminate, 30-40% of silica powder, 5-10% of alum stone and 5-10% of quicklime. The weight of water is 90%-95% of the total weight of the curing agent, silicate cement and silty clay, and can be 90%, 93% or 95%.

[0028] In this embodiment, among the curing agent, silicate cement and silty clay, the weight percentage of the curing agent can be 8%, 9% or 10%, the weight percentage of silicate cement can be 8%, 9%, 10%, 11% or 12%, and the weight percentage of silty clay can be 78%, 79%, 80%, 81%, 82%, 83% or 84%.

[0029] In the curing agent in this embodiment, the weight percentage of hemihydrate gypsum can be 8%, 9%, 10%, 11% or 12%, the weight percentage of calcium aluminate can be 40%, 41%, 42%, 43%, 44% or 45%, the weight percentage of silica powder can be 30%, 33%, 35%, 37%, 38% or 40%, the weight percentage of alum stone can be 5%, 6%, 7%, 8%, 9% or 10%, and the weight percentage of quicklime can be 5%, 6%, 7%, 8%, 9% or 10%.

[0030] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0031] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 1 or Example 2.

[0032] Embodiment 4: This embodiment provides a shield wall back grouting slurry, including water and the following weight percentages of components: 8% curing agent, 10% silicate cement and 82% silty clay. The curing agent includes the following weight percentages of components: 8% hemihydrate gypsum, 40% calcium aluminate, 40% silica powder, 5% alum stone and 7% quicklime. The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0033] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0034] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 2.

[0035] Embodiment 5: This embodiment provides a shield wall back grouting slurry, including water and the following weight percentages of components: 10% curing agent, 10% silicate cement and 80% silty clay. The curing agent includes the following weight percentages of components: 8% hemihydrate gypsum, 40% calcium aluminate, 40% silica powder, 5% alum stone and 7% quicklime. The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0036] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0037] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 2.

[0038] Embodiment 6: This embodiment provides a shield wall back grouting slurry, including water and the following weight percentages of components: 8% curing agent, 10% silicate cement and 82% silty clay. The curing agent includes the following weight percentages of components: 10% hemihydrate gypsum, 40% calcium aluminate, 35% silica powder, 5% alum stone, and 10% quicklime. The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0039] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0040] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 2.

[0041] Embodiment 7: This embodiment provides a shield wall back grouting slurry, including water and the following weight percentages of components: 10% curing agent, 10% silicate cement and 80% silty clay. The curing agent includes the following weight percentages of components: 10% hemihydrate gypsum, 40% calcium aluminate, 35% silica powder, 5% alum stone, and 10% quicklime. The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0042] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0043] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 2.

[0044] Embodiment 8: This embodiment provides a shield wall back grouting slurry, including water and the following weight percentages of components: 8% curing agent, 10% silicate cement and 82% silty clay. The curing agent includes the following weight percentages of components: 12% hemihydrate gypsum, 45% calcium aluminate, 30% silica powder, 8% alum stone and 5% quicklime. The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0045] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0046] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 2.

[0047] Embodiment 9: This embodiment provides a shield wall back grouting slurry, including water and the following weight percentages of components: 10% curing agent, 10% silicate cement and 80% silty clay. The curing agent includes the following weight percentages of components: 12% hemihydrate gypsum, 45% calcium aluminate, 30% silica powder, 8% alum stone, and 5% quicklime. The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

[0048] In this embodiment, the raw materials of the curing agent, silicate cement and silty clay are all in powder form.

[0049] A shield wall post-grouting slurry in this embodiment is prepared by the preparation method in Example 2.

[0050] The performance of the shield wall post-grouting slurry in the above Examples 4-9 was tested, and the test results are shown in Table 1 below.

[0051]

[0052] Table 1 As can be seen from Table 1, the initial setting time of the shield wall post-grouting slurry of Examples 4-9 is <10h, and the fluidity is good. In actual projects, the setting time can be adjusted by further adding a coagulant and changing the proportion according to the formation conditions and the excavation speed through field tests. For highly permeable formations and sections where grouting needs to provide higher early strength, the proportion can be further adjusted and early strength agents can be added through field tests to further shorten the setting time, obtain early strength, and ensure good grouting effects.

[0053] Under standard curing conditions, the indoor compressive strength of the shield wall post-grouting slurry of Examples 4-9 is not less than 1MPa within 24 hours and not less than 2.5MPa (slightly greater than the natural compressive strength of strongly weathered rock) after 28 days. The slurry stone rate is >95%, that is, the consolidation shrinkage rate is <5%. The slurry funnel viscosity is 25±3s, and the injectability is good.

[0054] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A shield wall back grouting slurry, comprising water, It is characterized in that The invention also comprises the following components in weight percentage: 8-10% of curing agent, 8-12% of silicate cement and 78-84% of silty clay, and the weight of water is 90%-95% of the total weight of the curing agent, silicate cement and silty clay.

2. A shield wall post-grouting slurry according to claim 1, It is characterized in that The weight percentages of the curing agent, silicate cement and silty clay are: 10% of the curing agent, 10% of the silicate cement and 80% of the silty clay.

3. A shield wall post-grouting slurry according to claim 1 or 2, It is characterized in that Curing agents include hemihydrate gypsum, calcium aluminate, silica powder, alunite and quicklime.

4. A shield wall post-grouting slurry according to claim 3, It is characterized in that The weight percentages of hemihydrate gypsum, calcium aluminate, silica powder, alunite and quicklime in the curing agent are as follows: 8-12% hemihydrate gypsum, 40-45% calcium aluminate, 30-40% silica powder, 5-10% alunite and 5-10% quicklime.

5. A shield wall post-grouting slurry according to claim 4, It is characterized in that The weight percentages of hemihydrate gypsum, calcium aluminate, silica powder, alunite and quicklime are as follows: 10% hemihydrate gypsum, 40% calcium aluminate, 35% silica powder, 5% alunite and 10% quicklime.

6. The shield wall post-grouting slurry according to claim 1, It is characterized in that The weight of water is 90% of the total weight of the curing agent, silicate cement and silty clay.

7. A method for preparing a grouting slurry for a shield wall. It is characterized in that The method for preparing a shield wall post-grouting slurry as claimed in any one of claims 1 to 6 comprises the following steps: adding water to the prepared curing agent, silicate cement and silty clay and stirring and mixing them.

8. A method for preparing a shield wall post-grouting slurry according to claim 7, It is characterized in that The preparation of the curing agent comprises the following steps: placing hemihydrate gypsum, calcium aluminate, silica powder, alum stone and quicklime in a mixing device, mixing and stirring for 3 to 5 minutes.

9. The method for preparing a shield wall post-grouting slurry according to claim 7, It is characterized in that The stirring speed of adding water and stirring mixing is 600-700 r / min, and the stirring time is 8-10 min.