Leveling agent applicable to high optical parts such as canopy, and preparation method and application thereof
Through the leveling agent with amphiphilic structure and high surface tension prepared in a protective atmosphere, the contradiction between the leveling time of the coating on the complex curvature surface and the surface drying time is solved, and the coating without optical defects is realized, and the cabin is improved Protective performance of cover.
Patent Information
- Application Number
- CN202411151218.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing paints are prone to optical defects on large-size and complex curvature surfaces, such as flow marks, ripple, etc., which leads to optical distortion, which cannot effectively resolve the contradiction between leveling time and surface drying time, affecting the protective performance of the coating.
The leveling agent prepared by reacting aliphatic isocyanate with functionalized ionic liquid in a protective atmosphere has an amphiphilic structure and a high surface tension, which can quickly migrate to the surface of the wet film, form a single molecular layer, reduce the coating leveling time, and avoid Photodistortion.
Fast leveling is achieved on complex curvature surfaces, and the prepared coating has no optical defects, which solves the contradiction between leveling time and surface drying time, and improves the leveling performance and protective effect of the coating.
Smart Images

Figure BDA0005003712990000101 
Figure BDA0005003712990000111 
Figure BDA0005003712990000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a leveling agent suitable for high optical parts such as cockpit covers, and a preparation method and application thereof. Background Art
[0002] The function of the aircraft canopy is to seal the cockpit, provide the pilot with a comfortable, closed, spacious and bright activity space, protect the pilot from the impact of the oncoming high-speed airflow and the invasion of the external environment, and provide the pilot with a good field of vision to complete various reconnaissance and combat missions. Modern aircraft canopies are mostly made of optical plastics. Compared with glass, they have many advantages, such as light weight, strong impact resistance, and low production cost. However, optical plastics also have obvious disadvantages: optical plastics are soft in texture and have poor scratch resistance. By coating a layer of wear-resistant polyurethane protective coating on the surface of organic glass, it can overcome its own shortcomings such as poor wear resistance and easy scratching.
[0003] However, as an optical component, the canopy protective coating has extremely high requirements for optical defect control. The presence of optical defects such as flow marks causes light distortion, which seriously affects the pilot's quick and accurate observation of the external environment and makes it impossible to effectively complete various operations and responses. Good optical leveling effect is a necessary condition for the protective coating to be applied to the canopy protection.
[0004] Currently, there is no optical coating specifically prepared for large-size optical parts. Existing coatings are applied on optical plexiglass, especially on large-size surfaces with complex curvatures, which can easily cause optical defects such as flow marks and ripples. More serious optical problems may also exist, such as shrinkage holes, orange peel, and sagging. Light deviates after passing through the optical defect coating, causing light distortion, thereby deforming the image and hindering the pilot's accurate judgment.
[0005] For curved optical coatings, the main problem currently is that the leveling time is greater than the flow time, and the coating cannot be sufficiently leveled, resulting in optical defects such as orange peel, ripples, and flow marks. To solve this problem, it is necessary to extend the flow time or reduce the leveling time. The preparation of optical coatings requires rapid surface drying after coating to reduce the risk of dust embedding. Extending the flow time also increases the surface drying time accordingly. On the other hand, if the flow time is too long, the thickness of the prepared coating is insufficient and cannot meet the use requirements of the protective coating. Therefore, the leveling problem cannot be solved simply by extending the flow time. Existing leveling agents are selected. Silicone leveling agents reduce surface tension and have a good wetting effect, but they cannot provide sufficient leveling power for high-viscosity wet films. The higher the surface tension of acrylic leveling agents, the higher the compatibility. They cannot quickly migrate to the surface of the wet film. Acrylic leveling agents that can migrate quickly have relatively low surface tension and cannot achieve a good leveling effect. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a leveling agent with an amphiphilic structure and high surface tension suitable for high optical parts such as cockpit covers, and a preparation method and application thereof.
[0007] The present invention provides a method for preparing a leveling agent suitable for high optical parts such as a canopy, comprising the following steps:
[0008] The aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent are mixed and reacted in a protective atmosphere to obtain a leveling agent.
[0009] Preferably, the cation in the functionalized ionic liquid comprises one or more of a hydroxyl group, an amino group and a carboxyl group;
[0010] The first catalyst is selected from tertiary amine catalysts and / or organic tin catalysts.
[0011] Preferably, the aliphatic isocyanate is selected from one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, HDI dimer and HDI trimer;
[0012] The functionalized ionic liquid is selected from one or more of 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-carboxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-hydroxyethyl-3-methylimidazolium chloride, 1-hydroxyethyl-3-methylimidazolium tetrafluoroborate, 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate, 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide and hydroxyethyl trimethylammonium trifluoromethanesulfonate;
[0013] The tertiary amine catalyst is selected from one or more of triethylamine, diethylenetriamine, dimethylhexadecylamine, triethylenediamine, triethanolamine, methyldiethanolamine, dimethylethanolamine and pyridine;
[0014] The organotin catalyst is selected from one or more of dibutyltin dilaurate, stannous octoate and triethylenediamine.
[0015] Preferably, the mass ratio of the aliphatic isocyanate to the functionalized ionic liquid is 1:(1-3).
[0016] Preferably, the mass of the first solvent is 40% to 60% of the total mass of the aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent;
[0017] The mass of the first catalyst is 0.01% to 0.05% of the total mass of the aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent.
[0018] Preferably, the reaction temperature is 60°C to 80°C; and the reaction time is 2 to 10 hours.
[0019] The present invention also provides a leveling agent prepared by the above preparation method, which is formed by the reaction of aliphatic isocyanate and functionalized ionic liquid.
[0020] The present invention also provides a polyurethane protective coating, comprising a leveling agent prepared by the above preparation method.
[0021] Preferably, the polyurethane protective coating comprises component A and component B;
[0022] The component A comprises a polyol polymer, a chain extender, a second catalyst, a second solvent, a leveling agent and a light stabilizer;
[0023] The B component includes an aliphatic diisocyanate.
[0024] Preferably, the mass of the leveling agent is 0.01% to 0.05% of the mass of the polyurethane protective coating.
[0025] The present invention provides a method for preparing a leveling agent, comprising the following steps: mixing and reacting aliphatic isocyanate, functionalized ionic liquid, a first catalyst and a first solvent in a protective atmosphere to obtain a leveling agent. Compared with the prior art, the leveling agent prepared by the present invention has an amphiphilic structure, can quickly migrate to the surface of a wet film, form a monomolecular layer on the surface of the film, and utilize its high surface tension to provide a leveling power for a high-viscosity wet film, thereby reducing the leveling time of the coating, making the leveling time close to or less than the flow time, solving the contradictory requirements of optical parts for the flow time of the coating, and making the coating prepared after coating have good leveling performance and no optical distortion.
[0026] The experimental results show that the polyurethane protective coating prepared using the leveling agent can quickly level on the surface of a cockpit cover with complex curvature. The prepared coating has no optical defects when projected at an angle greater than 15° and does not produce light distortion, thus solving the optical problem of applying the protective coating to the cockpit cover. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the leveling agent obtained in Example 1 of the present invention;
[0028] Figure 2 The diagram is a leveling effect diagram of the coatings obtained in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] The invention provides a method for preparing a leveling agent suitable for high optical parts such as a canopy, comprising the following steps: mixing and reacting aliphatic isocyanate, functionalized ionic liquid, a first catalyst and a first solvent in a protective atmosphere to obtain the leveling agent.
[0031] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.
[0032] In a specific embodiment provided by the present invention, the aliphatic isocyanate preferably includes but is not limited to one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, HDI dimer and HDI trimer. The use of aliphatic isocyanate can prevent yellowing during use.
[0033] In a specific embodiment provided by the present invention, the functionalized ionic liquid comprises a cation and an anion; the cation of the functionalized ionic liquid preferably comprises one or more of a hydroxyl group, an amino group and a carboxyl group; the anion of the functionalized ionic liquid is preferably bis(trifluoromethanesulfonyl)imide; in the present invention, most preferably, the functionalized ionic liquid includes but is not limited to one or more of 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-carboxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-hydroxyethyl-3-methylimidazolium chloride salt, 1-hydroxyethyl-3-methylimidazolium tetrafluoroborate, 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate, 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and hydroxyethyl trimethylammonium trifluoromethanesulfonate.
[0034] In a specific embodiment provided by the present invention, the first catalyst is preferably a tertiary amine catalyst and / or an organotin catalyst.
[0035] The tertiary amine catalyst can be any tertiary amine catalyst well known to those skilled in the art without any special limitation. In a specific embodiment provided by the present invention, the tertiary amine catalyst is preferably one or more of triethylamine, diethylenetriamine, dimethylhexadecylamine, triethylenediamine, triethanolamine, methyldiethanolamine, dimethylethanolamine and pyridine.
[0036] The organotin catalyst can be any organotin catalyst well known to those skilled in the art without any particular limitation. In a specific embodiment provided by the present invention, the organotin catalyst is preferably one or more of dibutyltin dilaurate, stannous octoate and triethylenediamine.
[0037] In a specific embodiment provided by the present invention, the mass ratio of the aliphatic isocyanate to the functionalized ionic liquid is preferably 1:(1-3), more preferably 1:(1.5-3); in some embodiments provided by the present invention, the mass ratio of the aliphatic isocyanate to the functionalized ionic liquid is specifically 1:2, 1:1.5 or 1:3.
[0038] In a specific embodiment provided by the present invention, the mass of the first catalyst is 0.01% to 0.05% of the total mass of the aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent, preferably 0.01% to 0.04%, more preferably 0.01% to 0.03%, and even more preferably 0.01% to 0.02%.
[0039] In a specific embodiment provided by the present invention, the first solvent can be an organic solvent well known to those skilled in the art without any special limitation. In the present invention, it preferably includes but is not limited to one or more of butyl acetate, cyclohexanone, dioxane and propylene glycol methyl ether propionate.
[0040] In a specific embodiment provided by the present invention, the mass of the first solvent is 40% to 60% of the total mass of the aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent, preferably 45% to 55%, and more preferably 50%.
[0041] The aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent are mixed and reacted in a protective atmosphere to obtain a leveling agent; the protective atmosphere can be any protective atmosphere well known to those skilled in the art without any special limitation, and nitrogen is preferably used in the present invention; the reaction temperature is preferably 60°C to 80°C, more preferably 65°C to 75°C, and more preferably 70°C; the reaction time is preferably 2 to 10 hours, more preferably 4 to 8 hours, more preferably 5 to 7 hours, and most preferably 6 hours.
[0042] The leveling agent prepared by the present invention has an amphiphilic structure, can quickly migrate to the surface of a wet film, form a monomolecular layer on the surface of the film, and use its high surface tension to provide leveling power for a high-viscosity wet film, thereby reducing the leveling time of the coating, making the leveling time close to the flow time or less than the flow time, solving the contradictory requirements of optical parts for the flow time of the coating, and making the coating prepared after coating have good leveling performance without generating optical distortion.
[0043] The present invention also provides a leveling agent prepared by the above preparation method, which is formed by the reaction of aliphatic isocyanate and functionalized ionic liquid.
[0044] In a specific embodiment provided by the present invention, the aliphatic isocyanate is selected from one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, HDI dimer and HDI trimer.
[0045] In a specific embodiment provided by the present invention, the functionalized ionic liquid preferably comprises a cation and an anion; the cation of the functionalized ionic liquid preferably comprises one or more of a hydroxyl group, an amino group and a carboxyl group; the functionalized ionic liquid preferably includes but is not limited to one or more of 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-carboxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-hydroxyethyl-3-methylimidazolium chloride salt, 1-hydroxyethyl-3-methylimidazolium tetrafluoroborate, 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate, 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and hydroxyethyl trimethylammonium trifluoromethanesulfonate.
[0046] In a specific embodiment provided by the present invention, the mass ratio of the aliphatic isocyanate to the functionalized ionic liquid is preferably 1:(1-3), more preferably 1:(1.5-3); in some embodiments provided by the present invention, the mass ratio of the aliphatic isocyanate to the functionalized ionic liquid is specifically 1:2, 1:1.5 or 1:3.
[0047] The invention obtains a novel leveling agent by reacting difunctional or trifunctional isocyanate with functionalized ionic liquid to block all NCO groups. The leveling agent has a large surface tension and is not completely miscible with the resin. It can form a monomolecular layer on the surface of the wet film and improve the surface flowability.
[0048] The present invention also provides a polyurethane protective coating, comprising the above-mentioned leveling agent.
[0049] The leveling agent prepared by the present invention can enhance the leveling power and the leveling effect, and can achieve high leveling of the coating without prolonging the surface drying time of the coating and without affecting the thickness of the coating.
[0050] In a specific embodiment provided by the present invention, the leveling agent is preferably 0.01% to 0.05% by mass of the polyurethane protective coating, more preferably 0.02% to 0.04%, further preferably 0.02% to 0.03%, and most preferably 0.02%.
[0051] In a specific embodiment provided by the present invention, the polyurethane protective coating includes component A and component B; the component A includes a polyol polymer, a chain extender, a second catalyst, a second solvent, a leveling agent and a light stabilizer; the component B includes an aliphatic diisocyanate.
[0052] The polyol polymer can be any polyol polymer well known to those skilled in the art without any special limitation. In a specific embodiment provided by the present invention, the polyol polymer preferably includes but is not limited to one or more of polycaprolactone diol, polycarbonate and polyether polyol, more preferably polycaprolactone diol PCL210N.
[0053] In a specific embodiment provided by the present invention, the mass of the polyol polymer is preferably 20% to 40% of the polyurethane protective coating, more preferably 25% to 35%, more preferably 28% to 35%, more preferably 30% to 33%, and most preferably 31% to 32%; in some embodiments provided by the present invention, the mass of the polyol polymer is specifically 31.56% of the polyurethane protective coating.
[0054] The chain extender can be any chain extender well known to those skilled in the art without any special limitation. In a specific embodiment provided by the present invention, the chain extender is preferably 1,2,4-butanetriol.
[0055] In a specific embodiment provided by the present invention, the mass of the chain extender is preferably 1% to 5% of the polyurethane protective coating, more preferably 1.5% to 4%, more preferably 2% to 3%, more preferably 2.3% to 2.6%, and most preferably 2.4% to 2.5%; in some embodiments provided by the present invention, the mass of the chain extender is specifically 2.47% of the mass of the polyurethane protective coating.
[0056] The second catalyst can be a catalyst well known to those skilled in the art, without special restrictions. In a specific embodiment provided by the present invention, the second catalyst is preferably a tertiary amine catalyst and / or an organotin catalyst. The tertiary amine catalyst can be a tertiary amine catalyst well known to those skilled in the art, without special restrictions. In a specific embodiment provided by the present invention, the tertiary amine catalyst is preferably one or more of triethylamine, diethylenetriamine, dimethylhexadecylamine, triethylenediamine, triethanolamine, methyldiethanolamine, dimethylethanolamine and pyridine. The organotin catalyst can be an organotin catalyst well known to those skilled in the art, without special restrictions. In a specific embodiment provided by the present invention, the organotin catalyst is preferably one or more of dibutyltin dilaurate, stannous octoate and triethylenediamine.
[0057] In a specific embodiment provided by the present invention, the mass of the second catalyst is preferably 0.01% to 2% of the polyurethane protective coating, more preferably 0.01% to 1.5%, further preferably 0.02% to 1%, further preferably 0.02% to 0.5%, further preferably 0.02% to 0.1%, further preferably 0.02% to 0.05%, and most preferably 0.03%.
[0058] The light stabilizer may be any light stabilizer known to those skilled in the art without any particular limitation. In the present invention, Tinuvin 770 is preferred.
[0059] In a specific embodiment provided by the present invention, the mass of the light stabilizer is preferably 0.1% to 1% of the mass of the polyurethane protective coating, more preferably 0.3% to 0.8%, further preferably 0.4% to 0.6%, and most preferably 0.5%.
[0060] The second solvent can be an organic solvent well known to those skilled in the art without any special limitation. In the present invention, butyl acetate and N,N-dimethylformamide are preferably used. The mass ratio of butyl acetate to N,N-dimethylformamide is preferably 1:(1-2), more preferably 1:(1.3-1.8), further preferably 1:(1.4-1.6), and most preferably 1:1.5.
[0061] In a specific embodiment provided by the present invention, the second solvent is preferably 40% to 60% of the mass of the polyurethane protective coating, more preferably 45% to 55%, further preferably 48% to 52%, and most preferably 49% to 50%.
[0062] In another specific embodiment provided by the present invention, the component A preferably further comprises a wetting agent; the type of the wetting agent can be any wetting agent well known to those skilled in the art, and there is no particular limitation. In the present invention, the wetting agent is preferably an organosilicon wetting agent, and more preferably an organosilicon wetting agent Silok-8035; the mass of the wetting agent is preferably 0.01% to 0.05% of the mass of the polyurethane protective coating, more preferably 0.02% to 0.04%, further preferably 0.02% to 0.03%, and most preferably 0.02%.
[0063] In another specific embodiment provided by the present invention, the component A preferably further comprises an antioxidant; the type of the antioxidant may be any antioxidant well known to those skilled in the art, and is not particularly limited. In the present invention, Irganox 1010 is preferred; the mass of the antioxidant is preferably 0.1% to 1% of the mass of the polyurethane protective coating, more preferably 0.2% to 0.8%, more preferably 0.2% to 0.6%, more preferably 0.2% to 0.4%, more preferably 0.2% to 0.3%, and most preferably 0.25%.
[0064] In another specific embodiment provided by the present invention, the component A preferably also includes a UV absorber; the type of the UV absorber can be any UV absorber well known to those skilled in the art, without any special restrictions, and UV-328 is preferred in the present invention; the mass of the UV absorber is preferably 0.1% to 1% of the mass of the polyurethane protective coating, more preferably 0.2% to 0.8%, more preferably 0.2% to 0.6%, more preferably 0.2% to 0.4%, more preferably 0.2% to 0.3%, and most preferably 0.25%.
[0065] The aliphatic diisocyanate may be any aliphatic diisocyanate known to those skilled in the art without any particular limitation. In the present invention, it preferably includes but is not limited to one or more of the trimer of hexamethylene diisocyanate, isophorone diisocyanate and 4,4'-dicyclohexylmethane diisocyanate.
[0066] In a specific embodiment provided by the present invention, the mass of the aliphatic diisocyanate is preferably 10% to 20% of the mass of the polyurethane protective coating, more preferably 12% to 18%, further preferably 14% to 16%, and most preferably 15% to 16%; in some embodiments provided by the present invention, the mass of the aliphatic diisocyanate is specifically 15.52% of the mass of the polyurethane protective coating.
[0067] The present invention also provides a method for preparing the above-mentioned polyurethane protective coating, comprising the following steps: mixing component A and component B, filtering, and standing to obtain the polyurethane protective coating; the mixing method can be a method well known to those skilled in the art and is not particularly limited, and is preferably stirring in the present invention; the mixing time is preferably 10 to 60 minutes, more preferably 20 to 50 minutes, more preferably 25 to 40 minutes, and most preferably 30 minutes; the filtration is preferably positive pressure filtration; the standing time is preferably 10 to 60 minutes, more preferably 20 to 50 minutes, more preferably 25 to 40 minutes, and most preferably 30 minutes.
[0068] The present invention also provides an application of the polyurethane protective coating as an optical coating.
[0069] The present invention also provides an application of the polyurethane protective coating as a canopy protective coating.
[0070] The polyurethane protective coating provided by the present invention is used in lens, automobile or high-speed railway glass protection and the like which have high requirements on optical properties.
[0071] In order to further illustrate the present invention, a leveling agent suitable for high optical parts such as a canopy, a preparation method thereof and an application thereof provided by the present invention are described in detail below in conjunction with embodiments.
[0072] The reagents used in the following examples are all commercially available.
[0073] Example 1
[0074] The preparation method of the optical leveling polyurethane protective coating comprises:
[0075] Step 1: prepare a leveling agent, the raw materials of which include, by weight: 16.81% hexamethylene diisocyanate, 33.18% 1-hydroxyethyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt, 50% cyclohexanone, and 0.01% dibutyltin dilaurate. Place the above raw materials in a reaction bottle at 70°C under nitrogen protection and stir for 6 hours to obtain a leveling agent.
[0076] The obtained leveling agent was analyzed by nuclear magnetic resonance, and its nuclear magnetic resonance hydrogen spectrum was obtained as follows: Figure 1 shown.
[0077]
[0078] Step 2: Applying a leveling agent to the polyurethane protective coating, the raw materials of which include by weight: 31.56% of polycaprolactone diol (PCL210N), 2.47% of 1,2,4-butanetriol, 0.03% of catalyst dibutyltin dilaurate, 0.02% of the leveling agent obtained in step 1, 0.02% of wetting agent Silok-8035, 0.25% of antioxidant Irganox1010, 0.25% of ultraviolet absorber UV-328, 0.25% of light stabilizer Tinuvin770, 19.82% of butyl acetate, 29.81% of N,N-dimethylformamide, and 15.52% of isophorone diisocyanate.
[0079] Step 3: Mix the components except isophorone diisocyanate in step 2, and then pour them into a stirred reactor with isophorone diisocyanate, control the temperature at 20°C to react for 2 hours, let it stand for 30 minutes to remove bubbles, and apply the coating to the plexiglass by vertical spray coating at 20°C. After leveling and surface drying for 2 to 6 hours, transfer the product to a forced air drying oven at 70°C for curing for 12 hours.
[0080] Example 2
[0081] Step 1: prepare a leveling agent, the raw materials of which include, by weight: 22.3% of dicyclohexylmethane diisocyanate, 27.68% of 1-hydroxyethyl-3-methylimidazolium chloride, 50% of butyl acetate, and 0.02% of dibutyltin dilaurate. Place the above raw materials in a reaction bottle at 70° C. under nitrogen protection and stir for 6 hours to obtain a leveling agent.
[0082]
[0083] Step 2: Applying a leveling agent to the polyurethane protective coating, the raw materials of which include by weight: 31.56% of polycaprolactone diol (PCL210N), 2.47% of 1,2,4-butanetriol, 0.03% of catalyst dibutyltin dilaurate, 0.02% of the leveling agent obtained in step 1, 0.02% of wetting agent Silok-8035, 0.25% of antioxidant Irganox1010, 0.25% of ultraviolet absorber UV-328, 0.25% of light stabilizer Tinuvin770, 19.82% of butyl acetate, 29.81% of N,N-dimethylformamide, and 15.52% of isophorone diisocyanate.
[0084] Step 3: Mix the components except isophorone diisocyanate in step 2, and then pour them into a stirred reactor with isophorone diisocyanate, control the temperature at 20°C to react for 2 hours, let it stand for 30 minutes to remove bubbles, and apply the coating to the plexiglass by vertical spray coating at 20°C. After leveling and surface drying for 2 to 6 hours, transfer the product to a forced air drying oven at 70°C for curing for 12 hours.
[0085] Example 3
[0086] Step 1: prepare a leveling agent, the raw materials of which include, by weight: 19.943% HDI trimer, 30.05% hydroxyethyltrimethylammonium trifluoromethanesulfonate, 50% butyl acetate, and 0.02% dibutyltin dilaurate. Place the above raw materials in a reaction bottle at 70° C. under nitrogen protection and stir for 6 hours to obtain a leveling agent.
[0087]
[0088] Step 2: Applying a leveling agent to the polyurethane protective coating, the raw materials of which include by weight: 31.56% of polycaprolactone diol (PCL210N), 2.47% of 1,2,4-butanetriol, 0.03% of catalyst dibutyltin dilaurate, 0.02% of the leveling agent obtained in step 1, 0.02% of wetting agent Silok-8035, 0.25% of antioxidant Irganox1010, 0.25% of ultraviolet absorber UV-328, 0.25% of light stabilizer Tinuvin770, 19.82% of butyl acetate, 29.81% of N,N-dimethylformamide, and 15.52% of isophorone diisocyanate.
[0089] Step 3: Mix the components except isophorone diisocyanate in step 2, and then pour them into a stirred reactor with isophorone diisocyanate, control the temperature at 20°C to react for 2 hours, let it stand for 30 minutes to remove bubbles, and apply the coating to the plexiglass by vertical spray coating at 20°C. After leveling and surface drying for 2 to 6 hours, transfer the product to a forced air drying oven at 70°C for curing for 12 hours.
[0090] Comparative Example 1
[0091] Commercial acrylic leveling agent BYK354 is applied to polyurethane protective coatings. The raw materials include, by weight: polycaprolactone diol (PCL210N) 31.56%, 1,2,4-butanetriol 2.47%, catalyst dibutyltin dilaurate 0.03%, BYK254 leveling agent 0.02%, wetting agent Silok-8035 0.02%, antioxidant Irganox 1010 0.25%, ultraviolet absorber UV-328 0.25%, light stabilizer Tinuvin 770 0.25%, butyl acetate 19.82%, N,N-dimethylformamide 29.81%, and isophorone diisocyanate 15.52%.
[0092] Step 3: Mix the components except isophorone diisocyanate in step 2, and then pour them into a stirred reactor with isophorone diisocyanate, control the temperature at 20°C to react for 2 hours, let it stand for 30 minutes to remove bubbles, and apply the coating to the plexiglass by vertical spray coating at 20°C. After leveling and surface drying for 2 to 6 hours, transfer the product to a forced air drying oven at 70°C for curing for 12 hours.
[0093] Comparative Example 2
[0094] Commercial silicone leveling agent BYK333 is applied to polyurethane protective coatings. The raw materials include, by weight: polycaprolactone diol (PCL210N) 31.56%, 1,2,4-butanetriol 2.47%, catalyst dibutyltin dilaurate 0.03%, BYK333 leveling agent 0.02%, wetting agent Silok-8035 0.02%, antioxidant Irganox 1010 0.25%, ultraviolet absorber UV-328 0.25%, light stabilizer Tinuvin 770 0.25%, butyl acetate 19.82%, N,N-dimethylformamide 29.81%, and isophorone diisocyanate 15.52%.
[0095] Step 3: Mix the components except isophorone diisocyanate in step 2, and then pour them into a stirred reactor with isophorone diisocyanate, control the temperature at 20°C to react for 2 hours, let it stand for 30 minutes to remove bubbles, and apply the coating to the plexiglass by vertical spray coating at 20°C. After leveling and surface drying for 2 to 6 hours, transfer the product to a forced air drying oven at 70°C for curing for 12 hours.
[0096] Figure 2 The leveling effect diagrams of the coatings obtained in Examples 1 to 3 and Comparative Examples 1 to 3 (photographs projected at a 30° angle on a slide), wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, (d) is Comparative Example 1, and (e) is Comparative Example 2.
[0097] Table 1 is the statistical results of the leveling effects of the coatings obtained in Examples 1 to 3 and Comparative Examples 1 to 3.
[0098] Table 1 Performance and leveling state of the embodiments and comparative examples
[0099] Light transmittance (PMM substrate) Adhesion Taber100 stroke haze increases after treatment Leveling state Example 1 92.12% 5B 0.36% Leveling Example 2 92.08% 5B 0.42% Leveling Example 3 92.04% 5B 0.44% Leveling Comparative Example 1 92.06% 5B 0.35% Shallow flow marks Comparative Example 2 92.05% 5B 0.38% Severe flow marks
[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a leveling agent suitable for high optical parts such as canopies, characterized in that: The following steps are involved: The aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent are mixed and reacted in a protective atmosphere to obtain a leveling agent.
2. The preparation method according to claim 1, characterized in that: The cation in the functionalized ionic liquid comprises one or more of a hydroxyl group, an amino group and a carboxyl group; The first catalyst is selected from tertiary amine catalysts and / or organic tin catalysts.
3. The preparation method according to claim 2, characterized in that: The aliphatic isocyanate is selected from one or more of hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, HDI dimer and HDI trimer; The functionalized ionic liquid is selected from one or more of 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-carboxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-hydroxyethyl-3-methylimidazolium chloride, 1-hydroxyethyl-3-methylimidazolium tetrafluoroborate, 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate, 1-hydroxyethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide and hydroxyethyl trimethylammonium trifluoromethanesulfonate; The tertiary amine catalyst is selected from one or more of triethylamine, diethylenetriamine, dimethylhexadecylamine, triethylenediamine, triethanolamine, methyldiethanolamine, dimethylethanolamine and pyridine; The organotin catalyst is selected from one or more of dibutyltin dilaurate, stannous octoate and triethylenediamine.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the aliphatic isocyanate to the functionalized ionic liquid is 1:(1-3).
5. The preparation method according to claim 1, characterized in that: The mass of the first solvent is 40% to 60% of the total mass of the aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent; The mass of the first catalyst is 0.01% to 0.05% of the total mass of the aliphatic isocyanate, the functionalized ionic liquid, the first catalyst and the first solvent.
6. The preparation method according to claim 1, characterized in that: The reaction temperature is 60° C. to 80° C.; the reaction time is 2 to 10 hours.
7. A leveling agent prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It is formed by the reaction of aliphatic isocyanates with functionalized ionic liquids.
8. A polyurethane protective coating, characterized in that: The invention relates to a leveling agent prepared by the preparation method according to any one of claims 1 to 6.
9. The polyurethane protective coating according to claim 8, characterized in that: The polyurethane protective coating comprises component A and component B; The component A comprises a polyol polymer, a chain extender, a second catalyst, a second solvent, a leveling agent and a light stabilizer; The B component includes an aliphatic diisocyanate.
10. The polyurethane protective coating according to claim 9, characterized in that: The mass of the leveling agent is 0.01% to 0.05% of the mass of the polyurethane protective coating.
Citation Information
Patent Citations
Preparation method of HDI-TDI (Hexamethylene Diisocyanate-Toluene Diisocynate) polyurethane tripolymer
CN103242254A
Pressure-sensitive adhesive composition, surface protective film, and optical member
CN104250538A
Surface protection film, method for manufacturing surface protection film, and optical member
CN105764689A
Silicone leveling agent capable of improving over-coating performance of coating, and application thereof
CN110128659A
Tertiary amine modifier of aliphatic isocyanate, preparation method of tertiary amine modifier and light-stable polyurethane foam
CN111057020A
Cited By
Antistatic polyurethane protective film as well as preparation method and application thereof
CN121203212A