High-refractive-index optical material containing isothiocyanate and preparation method thereof
Through the combined preparation method of isothiocyanate, isocyanate and thioether type cyclosulfur compound, the problems of low purity and high cost in the synthesis process of the existing isothiocyanate compound are solved, and the preparation of high refractive index optical materials is realized , meet the needs of high-end optical components.
Patent Information
- Application Number
- CN202411227016.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
AI Technical Summary
The existing synthesis process of isothiocyanate compounds has problems such as low monomer purity, low transparency, by-product generation, unstable raw material supply and high production costs, which is difficult to meet the needs of high-end optical components.
The combination preparation method of isothiocyanate, isocyanate and sulfide type cyclosulfur compound is adopted to prepare polyurethane optical materials with adjustable refractive index by adjusting component ratio and reaction conditions, and improve the refractive index by using aqueous organic reaction and phase transfer catalyst. Reaction efficiency and purity.
The preparation of high-refractive index optical materials is realized, the refractive index is adjustable in the range of 1.66~1.78, the light transmission ratio is >87%, and the Abbe number is >26, which reduces production costs and facilitates industrial scale.
Smart Images

Figure CN119039563A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis and preparation of polyurethane polymer optical materials, and particularly relates to a polyurethane optical material containing disubstituted phenyl diisothiocyanate and a preparation method thereof. Background Art
[0002] Polyurethane refers to a polymer containing carbamate groups (-NH-COO) in its molecular structure. It is mainly obtained by the polymerization reaction of isocyanates and compounds containing active hydrogen. Transparent polyurethane does not contain chromophores, does not produce microphase separation, and does not contain impurities. It overcomes the opacity of traditional polyurethane and has the characteristics of high light transmittance, high strength and good impact resistance. It is widely used in optical fields such as lenses, light filtering protection, LED lighting, automotive glass and window materials.
[0003] Lightweighting of optical systems means minimizing the curvature and thickness while ensuring the optical performance, so as to make the optical devices miniaturized, precise and lightweight. As one of the most important properties of polyurethane optical materials, it has been the focus of research at home and abroad in recent years. Improving the refractive index is an important means to achieve lightweighting. For example, Japan's Mitsui Chemicals uses trivalent thiol with mercapto (-SH) instead of hydroxyl to react with isocyanate to prepare a high-refractive-index polyurethane resin (product number MR), with a refractive index of 1.70; for another example, introducing sulfur atoms or high sulfur-containing groups into isocyanate to prepare isothiocyanate, with a refractive index of 1.74.
[0004] The following are some examples of methods for synthesizing isothiocyanate compound monomers.
[0005] ⑴ Synthesized with thiophosgene as raw material. Thiophosgene reacts with aliphatic amines or aromatic amines to generate isothiocyanates, but thiophosgene is a highly toxic and volatile liquid, which poses a great danger to the environment and production safety.
[0006]
[0007] ⑵Synthesized using substituted thiourea as raw material. Isothiocyanate is generated by the decomposition reaction of aromatic thiourea or disubstituted thiourea. The domestic supply is unstable and industrial-scale production is limited.
[0008]
[0009] (3) The tertiary alcohol is reacted with triphenylphosphine, 2,3-dichloro-5,6-dicyanobenzoquinone (DDQ) and N-tetra-n-butylammonium thiocyanate to prepare isothiocyanate. Solid reagents are expensive and difficult to mass produce.
[0010]
[0011] ⑷ Organic amine and carbon disulfide (CS 2) reacts with an organic base or an inorganic base to generate an N-alkyl dithiocarbamate intermediate, and synthesizes isothiocyanate with a desulfurization reagent. The desulfurization reagent used in the reaction has the problems of being expensive, toxic, and polluting the environment.
[0012]
[0013] ⑸ The Lawesson reagent is reacted with isocyanate to synthesize isothiocyanate under microwave radiation, with a yield of up to 50%. This method does not require solvents and has the advantages of low pollution and fast reaction speed, but the Lawesson reagent used is relatively expensive, resulting in high production costs and affecting industrial promotion.
[0014]
[0015] (6) In the reaction of primary amine and carbon disulfide to synthesize isothiocyanate, tert-butyl carbonate diethyl phosphoric anhydride is used instead of the desulfurization reagent to synthesize isothiocyanate. This method has low product purity and produces too much azo color-producing substances during the reaction, resulting in low transparency and affecting the scope of use.
[0016]
[0017] The isothiocyanate compounds synthesized by the above chemical reactions generally have low S content or are accompanied by the production of other substances, including raw materials, by-products, solvents, etc., which coexist in the reaction system. Some substances generate by-products such as azo-structured chromophores during the reaction, resulting in low monomer purity and low transparency, which affects the application in the optical field; some have the defect of haze after cross-linking and curing, resulting in reduced transparency of the resin, which affects the use in the field of high-end optical components; some have problems such as harsh synthesis process conditions and unavailability of raw materials, making large-scale production difficult. Therefore, advanced synthesis technology will show its importance in the preparation of organic compounds. Summary of the invention
[0018] In view of the above problems of the prior art, the present invention provides a method for preparing a high refractive index optical material containing isothiocyanate. The polyurethane precursor material used to prepare the high refractive index optical material comprises three components A, B and C, wherein component A is an isothiocyanate and an isocyanate composition, with a content of 25 to 60 wt%; component B is a thiol compound with a refractive index of 1.56 to 1.80, with a content of 5 to 30 wt%; component C is a thioether-type episulfide compound containing 4 to 6 sulfur atoms, with a content of 15 to 50 wt%. By adjusting the content of isothiocyanate and episulfide compounds, a polyurethane precursor material with a required refractive index can be obtained. When used, the components are mixed and then subjected to polymerization reaction to prepare a polyurethane polymer optical material with an adjustable refractive index. The optical material has a visible light transmittance of >87%, an Abbe number of >26, and a refractive index that can be adjusted within the range of 1.66 to 1.78, providing a wider range of material selection for the application of high-end optical components.
[0019] To achieve the above object, the present invention provides the following technical solutions: A method for preparing a high-refractive-index optical material containing isothiocyanate, the method comprising the following steps: (1) Prepare polyurethane precursor materials, the composition and weight percentage of each component are as follows: Component A: isocyanate and isothiocyanate composition, 25-60 wt%; Wherein, the isothiocyanate is selected from at least one of the following compounds:
[0020] The weight ratio of isocyanate to isothiocyanate is (0.5~3):(1~3); Component B: thiol compound with a refractive index of 1.56 to 1.80, 5 to 30 wt%; Component C: 15-50 wt% of a thioether type episulfide compound containing 4-6 sulfur atoms; (2) Prepolymerization: Mix the components of step (1) above, add the additives and catalysts under stirring, prepolymerize at 50-80°C for 10-60 min, remove bubbles under vacuum, and inject into a mold; (3) Cross-linking and curing: The mold containing the prepolymer obtained in step (2) is placed in a curing furnace, heated to 35-55°C for 2-10 hours, then gradually raised to 80-100°C, and allowed to stand for 2-3 hours. Finally, it is cooled to room temperature and demolded to obtain a high refractive index optical material.
[0021] In the preparation method as described above, preferably, the auxiliary agent is triethylenediamine, and the weight percentage of triethylenediamine to isothiocyanate is (0.05-0.2):(1-5).
[0022] In the preparation method as described above, preferably, the catalyst is dibutyltin dilaurate or stannous isooctanoate, and the amount of the catalyst added is 1-3 wt % of the total amount of the polyurethane precursor material.
[0023] In the preparation method as described above, preferably, the thioether-type episulfide compound is selected from at least one of the following compounds:
[0024] (I)
[0025] (II) Where R is H or CH 3
[0026] (III) Among them, R 1 , R 2 , R 3 The same or different, each is OH or CH 3 .
[0027] In the preparation method as described above, preferably, the isocyanate is selected from one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), meta-xylylene diisocyanate (XDI), diphenylmethane diisocyanate (MDI), phorone diisocyanate (IPDI) and dicyclohexylmethane diisocyanate (HMDI).
[0028] In the preparation method as described above, preferably, the thiol is a polythiol compound containing more than two thiol groups, selected from: 2,5-dimercaptomethyl-1,4-dithiacyclohexane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithiacyclohexane, ethylene glycol bis(3-mercaptopropionate), 4,6-bis(mercaptomethylthio)1,3-dithiacyclohexane, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, etc., at least one of the following.
[0029] In the method as described above, preferably, the component A also includes a non-polar solvent, and the added amount is 1-3% of the weight of the isothiocyanate; more preferably, the non-polar solvent is selected from one or a mixed solvent of two or more selected from acetone, ethyl acetate, dichloromethane, chloroform, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide.
[0030] In another aspect, the present invention provides an isothiocyanate-containing high refractive index optical material, which is prepared by the method as described above.
[0031] In another aspect, the present invention provides a high refractive index optical material with a refractive index of 1.66 to 1.74, which is prepared by the method described above; wherein: Component A: isocyanate and isothiocyanate composition, 25-40wt%; Component B: thiol compound with a refractive index of 1.56 to 1.80, 5 to 30 wt%; Component C: 15-50 wt% of thioether-type episulfide compounds containing 4-6 sulfur atoms.
[0032] In another aspect, the present invention provides a high refractive index optical material with a refractive index of 1.75 or above, which is prepared by the method as described above; wherein: Component A: isocyanate and isothiocyanate composition, 40-60wt%; Component B: thiol compound with a refractive index of 1.56 to 1.80, 5 to 30 wt%; Component C: 15-50 wt% of thioether-type episulfide compounds containing 4-6 sulfur atoms.
[0033] The isothiocyanate of the present invention can be prepared by the following method: ⑴ Substitution reaction: Add thiocyanate to a reaction vessel containing distilled water, add dichloromethylbenzene and an organic solvent with a boiling point below 70°C in sequence with stirring, add a phase transfer catalyst dropwise, and control the temperature to 50-85°C during the reaction. 2 Protection reaction 1.5~3h; ⑵ Extraction and purification: Extract the organic layer with chloroform, add the adsorbent decolorant while stirring, let stand to separate the layers, and filter to remove the adsorbent decolorant; ⑶ Isomerization reaction: Distill off the organic solvent and cool to obtain a viscous transparent liquid, i.e., the isothiocyanate compound monomer.
[0034] The specific reaction formula is as follows:
[0035]
[0036] In the above-mentioned method for preparing isothiocyanate, preferably, the thiocyanate is one of potassium thiocyanate, sodium thiocyanate and ammonium thiocyanate; and the organic solvent is at least one of methanol, ether, n-pentane and acetone.
[0037] In the above-mentioned method for preparing isothiocyanate, preferably, the phase transfer catalyst is ethanolamine, and the amount of ethanolamine added is 1-3 wt % of the solvent.
[0038] In the above-mentioned method for preparing isothiocyanate, preferably, the adsorption decolorizing agent is attapulgite or diatomaceous earth, and the particle size is 50-300 mesh, preferably 100 mesh.
[0039] The synthesis of isothiocyanate in the present invention is an aqueous phase organic reaction. Through a phase transfer catalyst, thiocyanate can fully react with dichlorobenzene in the organic phase. 2 The metal ions in the group-substituted isothiocyanate form coordination with the thiocyanate ion (SCN-); the reaction is accompanied by heat release, and the temperature of the system needs to be controlled during the process. If the system temperature is too high, side reactions such as azo chromophores or self-polymerization of the system will occur during the reaction, seriously affecting the transparency and transmittance of the product; if the temperature is too low, the reaction rate will be low, which will lead to a long reaction time. At the same time, the distillation heat is used to convert -SCN to -NCS to achieve isomerization transposition; the alcohol solvent in the system cannot react with the generated isothiocyanate product due to the low temperature reaction, and the generation of thiocarbamate byproducts is strictly controlled, while the reaction time is minimized and the concentration of alcohol in the system is reduced; despite the above-mentioned improvement measures taken during the reaction, it is still difficult to avoid the generation of a small amount of miscellaneous ions and byproducts, and finally an adsorbent is used for physical removal.
[0040] The polyurethane precursor material with adjustable refractive index of the present invention comprises three components A, B and C. The isothiocyanate in the component A is a PS-1 to PS-3 compound, which has an ultra-high refractive index of 1.74 to 1.75. The isocyanate in the component A functions to make the polyurethane precursor material system uniform, and the isocyanate can accelerate the polymerization rate of the precursor material. The component C is an episulfide compound containing 4 to 6 sulfur atoms, especially a compound of formula I to formula III, which has a medium-high / ultra-high refractive index of 1.71 to 1.80. The addition of the episulfide compound can cooperate with the isothiocyanate to selectively adjust the refractive index of the optical material.
[0041] The beneficial effects of the present invention are: (1) The method of the present invention obtains a high refractive index optical material with a set refractive index by controlling the addition amount of each component.
[0042] (2) In the synthesis of the isothiocyanate of the present invention, the reactants are in a homogeneous phase, and the thiocyanate can fully contact with di(chloromethyl)benzene in the organic phase, so that the reaction is more complete. The low-temperature reaction is adopted to control the by-products in the reaction process, and the low-boiling point organic solvent is convenient for subsequent distillation, and the monomer transparency is high.
[0043] (3) The method of the present invention has simple reaction conditions, and the material composition and preparation process are simple, which reduces the application cost to a certain extent and facilitates industrial-scale development.
[0044] (4) The high refractive index optical material prepared by the method of the present invention has a visible light transmittance of >87%, an Abbe number >26, and a refractive index that can be adjusted within the range of 1.66 to 1.78, providing a wider range of material selection for the application of high-end optical components. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 FT-IR infrared spectrum of the isothiocyanate (PS-1) prepared in a specific embodiment.
[0047] Figure 2 The HNMR nuclear magnetic resonance hydrogen spectrum of the isothiocyanate (PS-1) prepared in the specific embodiment.
[0048] Figure 3 is the EI mass spectrum of the isothiocyanate (PS-2) prepared in a specific embodiment. DETAILED DESCRIPTION
[0050] 1. Sources and preparation methods of some raw materials in the following examples 1. Preparation of isothiocyanate compound (PS-1): 450g of sodium thiocyanate was added to a reaction vessel containing 48kg of distilled water, and 580g of p-dichloromethylbenzene and 5.2kg of methanol were added in sequence with stirring, and 65g of ethanolamine was added dropwise. The reaction temperature was controlled at 65°C, and N 2 The reaction was protected for 1.5 hours; the organic layer was extracted with chloroform, 25 g of attapulgite was added with stirring, and the chloroform in the organic layer was distilled off to obtain 625 g of isothiocyanate compound (PS-1), with a yield of 75.7%.
[0051] Infrared spectra such as Figure 1 As shown, FT-IR (cm -1 ) Analysis: 3065 cm -1 The benzene ring CH stretching vibration peak appears at 2151 cm -1 The characteristic peak of N=C=S antisymmetric stretching vibration is 1590cm -1 The C=N bending vibration peak appears at 1274 cm-1 The CN stretching vibration peak appears at 1170 cm -1 A C=S stretching vibration peak appears at .
[0052] HNMR nuclear magnetic resonance hydrogen spectrum, such as Figure 2 As shown, 1 H NMR (δ) analysis: δ = 4.16 ppm is the characteristic peak of the methylene group connected to -NCS, and δ = 7.26 ~ 7.44 ppm is the H atom peak on the benzene ring.
[0053] 2. Preparation of isothiocyanate compound (PS-2): 450g of sodium thiocyanate was added to a reaction vessel containing 46kg of distilled water, 550g of m-dichloromethylbenzene and 4.8kg of methanol were added in sequence with stirring, and 60g of ethanolamine was added dropwise. The reaction temperature was controlled at 65°C and N 2 The reaction was protected for 1.5 hours; the organic layer was extracted with chloroform, 25 g of attapulgite was added with stirring, and the chloroform in the organic layer was distilled off to obtain 610 g of isothiocyanate compound (PS-2) with a yield of 77.2%.
[0054] Infrared spectrum FT-IR (cm -1 ) Analysis: 3065 cm -1 The CH stretching vibration peak of the benzene ring appears at 2150 cm -1 The characteristic peak of N=C=S antisymmetric stretching vibration is 1593cm -1 The C=N bending vibration peak appears at 1275 cm -1 The CN stretching vibration peak appears at 1172cm -1 A C=S stretching vibration peak appears at .
[0055] EI mass spectrum Figure 3 As shown, the electron energy is 70 eV, the scanning mode is full scan, and the scanning mass range is 50-300 m / z. The EI mass spectrum of the target product isothiocyanate is compared with the EI standard mass spectrum to determine the structure. The fragment ion peak m / z is 115 (M + ), 100, 72, 57.
[0056] 3. Preparation of tetracyclic sulfide compounds (compounds of formula I)
[0057] (I) Add 900g of 1,3-diphenylacetone and 1680g of anhydrous ethanol to the reaction vessel, stir evenly, and then introduce hydrogen sulfide and hydrogen chloride dry gas for 6h. The reaction temperature is controlled at 2°C. After 10h, the precipitate is vacuum dried to obtain a thiol intermediate. Take 360g of the thiol intermediate and add it to 1100g of ethanol. After dissolving, add 820g of ferric chloride and 650g of water and stir repeatedly. The temperature is controlled at 5°C and the reaction is carried out for 4.5h. The collected precipitate is recrystallized with n-hexane and vacuum dried to obtain 184g of tetracyclic sulfur compound (II) with a yield of 51.4%.
[0058] 4. Preparation of pentacyclic sulfur compounds (compounds of formula II):
[0059] (ii) Dissolve 2200g of sodium sulfide in 11000g of anhydrous ethanol, add 2400g of carbon disulfide, control the reaction under stirring at room temperature, add 160g of sulfur under stirring, react at 45°C for 50min, cool naturally to room temperature, add n-pentane solvent to precipitate sodium pentathiocarbonate. Take 1050g of sodium pentathiocarbonate and add 2400g of methanol. After dissolving, heat to 35°C, add 5200g of 8% dibromomethane methanol solution dropwise within 2h, react under stirring for 31h, add distilled water, extract with chloroform, combine the extracts, dry over anhydrous sodium sulfate, and remove chloroform under atmospheric distillation to obtain 318g of pentacyclic sulfur compound (ii) with a yield of 45.4%.
[0060] 5. Preparation of hexacyclic sulfur compounds (compounds of formula III):
[0061] (iii) 3100 g of sodium pentathiocarbonate was added to 83500 g of methanol, and the temperature was raised to 30°C. 1650 g of 1,3-dimercaptoisopropanol was added, and the reaction was slowly stirred for about 2 hours. 2500 g of purified water and 2400 g of chloroform were added thereto. The aqueous layer was separated and the extracts were combined. Anhydrous sodium sulfate was added to dry the extracts. The extracts were filtered and the solvent was evaporated at 60°C. The viscous compound after distillation was dissolved in pyridine solvent, the insoluble matter was removed by filtration, and the solvent was recovered under reduced pressure to obtain 1820 g of hexacyclic sulfur compound (iii) with a yield of 38.5%.
[0062] 6. Refractive index of isocyanate and isothiocyanate and their sources By testing the refractive index of each component monomer, the refractive index value range is divided into: nd≥1.74 is an ultra-high refractive index, nd=1.64~1.74 is a high refractive index range, nd=1.54~1.64 is a medium-high refractive index range, and nd≤1.54 is a medium-low refractive index, as shown in Table 1 and Table 2 below.
[0063]
[0064]
[0065] 2. Embodiment The following is a further description of the present invention through specific embodiments, but it is not intended to limit the protection scope of the present invention.
[0066] Example 1: Preparation of 1.67 refractive index polyurethane polymer optical material Heat 65g of isothiocyanate (PS-1) to 70°C, add 65g of m-phenylenedimethyl isocyanate, stir evenly to form a mixture, and then add 55g of 2,3-dithio(mercaptoethyl)-propane and 95g of pentasulfur heterocycle (Formula ii) to the mixture to obtain a prepolymer. Stir and add 2g of triethyldiamine and 6.5g of dibutyltin dilaurate to the prepolymer, heat to 60°C for prepolymerization for 45 minutes, vacuum degassing, and inject into a tempered mold with a refractive index of 500 degrees. Place the mold containing the prepolymer in a curing oven at 50°C for 6h, heat to 90°C, continue to place for 2.5h, and finally cool to room temperature for demolding to obtain a 1.67 refractive index polyurethane polymer optical material.
[0067] Example 2: Preparation of 1.69 refractive index polyurethane polymer optical material Heat 75g of isothiocyanate (PS-1) to 70°C, add 60g of diphenylmethane diisocyanate, stir evenly to form a mixture, and then add 35g of 2,3-dithio (mercaptoethyl)-propane and 115g of tetrasulfide heterocycle (Formula I) to the mixture to obtain a prepolymer. Stir and add 2g of triethyldiamine and 6.5g of dibutyltin dilaurate to the prepolymer, heat to 60°C for prepolymerization for 45 minutes, vacuum degassing, and inject into a tempered mold with a refractive index of 500 degrees. Place the mold containing the prepolymer in a curing oven at 50°C for 6h, heat to 90°C, continue to place for 2.5h, and finally cool to room temperature for demolding to obtain a 1.69 refractive index polyurethane polymer optical material.
[0068] Example 3: Preparation of 1.71 refractive index polyurethane polymer optical material Heat 90g of isothiocyanate (PS-1) to 70°C, add 40g of hexamethylene diisocyanate, stir evenly to form a mixture, and then add 20g of 2,3-dithio(mercaptoethyl)-propane and 130g of pentasulfur heterocycle (Formula ii) to the mixture to obtain a prepolymer. Stir and add 2g of triethyldiamine and 6.5g of dibutyltin dilaurate to the prepolymer, heat to 60°C for prepolymerization for 45 minutes, vacuum degassing, and inject into a tempered mold with a refractive index of 500 degrees. Place the mold containing the prepolymer in a curing oven at 50°C for 6h, heat to 90°C, continue to place for 2.5h, and finally cool to room temperature for demolding to obtain a 1.71 refractive index polyurethane polymer optical material.
[0069] Example 4: Preparation of 1.73 refractive index polyurethane polymer optical material Heat 65g of isothiocyanate (PS-1) to 70°C, add 60g of toluene diisocyanate, stir evenly to form a mixture, and then add 25g of 2,3-dithio (mercaptoethyl)-propane and 115g of hexasulfide heterocycle (Formula iii) to the mixture to obtain a prepolymer. Stir and add 2g of triethyldiamine and 6.5g of dibutyltin dilaurate to the prepolymer, heat to 60°C for prepolymerization for 45 minutes, vacuum degassing, and inject into a tempered mold with a refractive index of 500 degrees. Place the mold containing the prepolymer in a curing oven at 50°C for 6h, heat to 90°C, continue to place for 2.5h, and finally cool to room temperature for demolding to obtain a polyurethane polymer optical material with a refractive index of 1.73.
[0070] Example 5: Preparation of 1.75 refractive index polyurethane polymer optical material Heat 70g of isothiocyanate (PS-2) to 70°C, add 35g of diphenylmethane diisocyanate, stir evenly to form a mixture, and then add 10g of 2,3-dithio (mercaptoethyl)-propane and 110g of hexasulfide heterocycle (Formula iii) to the mixture to obtain a prepolymer. Stir and add 2g of triethyldiamine and 6.5g of dibutyltin dilaurate to the prepolymer, heat to 60°C for prepolymerization for 45 minutes, vacuum degassing, and inject into a tempered mold with a refractive index of 500 degrees. Place the mold containing the prepolymer in a curing oven at 50°C for 6h, heat to 90°C, continue to place for 2.5h, and finally cool to room temperature for demolding to obtain a 1.75 refractive index polyurethane polymer optical material.
[0071] Example 6: Preparation of 1.78 refractive index polyurethane polymer optical material Heat 95g of isothiocyanate (PS-2) to 70°C, add 15g of 2,3-dithio-1-propanethiol and 95g of hexasulfide heterocycle (Formula iii) with stirring to obtain a prepolymer. Stir and add 2.5g of triethyldiamine and 6.5g of dibutyltin dilaurate to the prepolymer, heat to 60°C for prepolymerization for 45 minutes, vacuum degassing, and inject into a tempered mold with a refractive index of 500 degrees. Place the mold containing the prepolymer in a curing oven at 50°C for 6h, heat to 90°C, continue to place for 2.5h, and finally cool to room temperature for demolding to obtain a polyurethane polymer optical material with a refractive index of 1.78.
[0072] 3. Optical performance test of the samples in the embodiment The optical properties of the prepared isothiocyanate compound and the polyurethane polymer optical material prepared in the example were tested respectively. Light transmittance is one of the most important properties of optical materials, which is expressed by transmittance (transmittance). The test was performed using the UV-8000 ultraviolet visible photometer of Shanghai Yuanxi Instrument Co., Ltd.; the refractive index and Abbe number were tested using the WZS1 Abbe refractometer of Shanghai Optical Instrument Equipment Co., Ltd. The test results are shown in Table 3.
[0073]
[0074] From the above test results, it can be seen that the isothiocyanate compound synthesized by the present invention has good light transmittance and a refractive index of 1.74; the isothiocyanate is compounded with isocyanate and episulfide compound to form a composition with different refractive indices, and then polymerized with a thiol compound monomer to prepare a polyurethane polymer optical material whose refractive index can be adjusted according to design requirements. The optical material has a visible light transmittance of more than 87%, an Abbe number of more than 26, and a refractive index that is adjustable within the range of 1.66 to 1.78.
Claims
1. A method for preparing a high refractive index optical material containing isothiocyanate, characterized in that: The method comprises the following steps: (1) Prepare polyurethane precursor materials, the composition and weight percentage of each component are as follows: Component A: isocyanate and isothiocyanate composition, 25-60 wt%; Wherein, the isothiocyanate is selected from at least one of the following compounds:
2. The weight ratio of isocyanate to isothiocyanate is (0.5~3):(1~3); Component B: thiol compound with a refractive index of 1.56 to 1.80, 5 to 30 wt%; Component C: 15-50 wt% of a thioether type episulfide compound containing 4-6 sulfur atoms; (2) Prepolymerization: Mix the components of step (1) above, add the additives and catalysts under stirring, prepolymerize at 50-80°C for 10-60 min, remove bubbles under vacuum, and inject into a mold; (3) Cross-linking and curing: The mold containing the prepolymer obtained in step (2) is placed in a curing furnace, heated to 35-55°C for 2-10 hours, then gradually raised to 80-100°C, and allowed to stand for 2-3 hours. Finally, it is cooled to room temperature and demolded to obtain a high refractive index optical material.
3. The preparation method according to claim 1, characterized in that: The auxiliary agent is triethylenediamine, and the weight percentage of triethylenediamine to isothiocyanate is (0.05-0.2): (1-5).
4. The preparation method according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate or stannous isooctanoate, and the amount of the catalyst added is 1-3 wt% of the total amount of the polyurethane precursor material.
5. The preparation method according to any one of claims 1 to 3, characterized in that The thioether type episulfide compound is selected from at least one of the following compounds: 6.(I) 7. (II) Where R is H or CH3 8. (III) in, R1, R2, and R3 are the same or different, and are each OH or CH3.
9. The preparation method according to claim 4, characterized in that: The isocyanate is selected from one of toluene diisocyanate, hexamethylene diisocyanate, meta-xylylene diisocyanate, diphenylmethane diisocyanate, phorone diisocyanate and dicyclohexylmethane diisocyanate.
10. The preparation method according to claim 4, characterized in that: The thiol is a polythiol compound containing two or more thiol groups, and is selected from: 2,5-dimercaptomethyl-1,4-dithiacyclohexane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithiacyclohexane, ethylene glycol bis(3-mercaptopropionate), 4,6-bis(mercaptomethylthio)1,3-dithiacyclohexane, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, etc., at least one of the following.
11. A high refractive index optical material containing isothiocyanate, characterized in that: The invention relates to a method for preparing the present invention.
12. A high refractive index optical material with a refractive index of 1.66 to 1.74, characterized in that: It is prepared by the method as described in any one of claims 1 to 6; wherein, Component A: isocyanate and isothiocyanate composition, 25-40wt%; Component B: thiol compound with a refractive index of 1.56 to 1.80, 5 to 30 wt%; Component C: 15-50 wt% of thioether-type episulfide compounds containing 4-6 sulfur atoms.
13. A high refractive index optical material having a refractive index of 1.75 or above, characterized in that: It is prepared by the method as described in any one of claims 1 to 6; wherein, Component A: isocyanate and isothiocyanate composition, 40-60wt%; Component B: thiol compound with a refractive index of 1.56 to 1.80, 5 to 30 wt%; Component C: 15-50 wt% of thioether-type episulfide compounds containing 4-6 sulfur atoms.
Citation Information
Cited By
Preparation method of pentaerythritol tetrathiol carboxylate composition
CN120485298A
Preparation method of pentaerythritol tetramercaptocarboxylate composition
CN120485298B
Engine wire harness with good shielding property and preparation method thereof
CN120590777A