Modified polyolefin material as well as preparation method and application thereof
By blending polypropylene, ultra-high molecular weight polyethylene and other components in a twin-screw extruder, modified polyolefin materials with clear texture, high gloss and excellent mechanical properties are prepared. This solves the problems of insufficient performance and low production efficiency of existing modified polypropylene materials in imitating natural stone, and realizes the preparation of efficient and environmentally friendly imitation earth and stone materials.
Patent Information
- Application Number
- CN202411240015.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-29
AI Technical Summary
Existing modified polypropylene materials have problems in imitating natural stone, such as poor mechanical properties, scratch resistance and texture, insufficient gloss and texture, and high energy consumption and low production efficiency in the preparation process.
Modified polyolefin materials are prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, glitter powder, surfactant, antioxidant, and lubricant in a twin-screw extruder with a specific screw structure. The compatibilizer and surfactant are combined to improve the compatibility of inorganic and organic materials, and the use of a specific twin-screw extruder reduces energy consumption.
Modified polyolefin materials with clear texture, natural uneven surface, high gloss, and excellent mechanical properties were prepared. These materials are low in odor, environmentally friendly, and have high production efficiency, effectively improving the scratch resistance and imitation soil and stone effect of the materials.
Smart Images

Figure CN119039702A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and in particular to a modified polyolefin material and a preparation method and application thereof. Background Art
[0002] Marble, quartz, ceramics, clay and other natural stones or fired earth and stone materials are widely used in life and industry. Natural stone and earth and stone have strong rigidity, strong pressure resistance, good fire resistance, low expansion and contraction rate, and relatively stable properties. They are very common in the fields of home decoration and construction. However, the price of natural stone is relatively high and it is non-renewable. Clay, ceramics and other materials also have the problems of being fragile, complex processing procedures, high energy consumption, low processing efficiency and high transportation costs. Therefore, currently, imitation earth and stone materials with natural texture, excellent performance, environmental protection and low cost are often prepared by plastic materials to replace natural stone and earth and stone. The general imitation earth and stone materials are polypropylene materials.
[0003] As one of the five general-purpose plastics, polypropylene is lightweight, environmentally friendly, recyclable, cheap, and widely available. It is widely used in the fields of automobiles, home appliances, medical care, gardening, agriculture, clothing, etc. The method of modifying polypropylene for use as imitation soil and stone materials not only reduces the process of plastic spraying to achieve imitation soil and stone materials, reduces production energy consumption and costs, but also achieves 100% recyclability, providing support for the green and sustainable development of the industry. According to the different functional requirements of various fields, polypropylene can be improved through different modification methods to improve its required performance. The commonly used methods of polypropylene modification are compounding, cross-linking and additive modification.
[0004] CN104448569B discloses a marble-like spray-free polypropylene composite material and a preparation method and application thereof. The technical solution is to add glass fiber, speckled black pigment and other additives to polypropylene, and then blend them through a twin-screw extruder, and melt extrude to obtain the marble-like spray-free polypropylene composite material. However, the technical solution requires a large amount of glass fiber to be added. Because the glass fiber has a needle-like structure, the speckled black pigment cannot be evenly dispersed in the system, so that the surface reflectivity of the material is poor, which is very different from the texture of natural stone.
[0005] CN108559175B discloses a spray-free polypropylene material with marble black and white texture and a preparation method thereof. The technical solution controls the generation of the black and white texture of the material by adding black masterbatch and white masterbatch to the polypropylene material, and adjusting the ratio of the black masterbatch and the white masterbatch in the system and the temperature during injection molding. Although the operation method in the technical solution is simple and can achieve the texture of imitating natural stone, the wear resistance is poor, and the actual material has a strong plastic feeling and lacks three-dimensional sense.
[0006] CN112480530A discloses a low-floating fiber marble effect reinforced polypropylene modified material and a preparation method thereof. This technical solution achieves a dark texture effect of the material by adding dark polyester fiber, glass fiber, compatibilizer and processing aid into polypropylene. This technical solution has a good imitation marble appearance, but the texture lacks three-dimensional sense and has high requirements on the mold structure and injection molding machine.
[0007] CN112210153B discloses a radiation-crosslinkable ceramic polyolefin material and a preparation method thereof. The technical scheme prepares the radiation-crosslinkable ceramic polyolefin material by melt-mixing polyolefin, ceramic functional masterbatch, inorganic filler, radiation sensitizer, stabilizer and processing aid. The preparation process is complicated, the production efficiency of the ceramic functional masterbatch is low, and it cannot be recycled during use.
[0008] In summary, in order to replace natural stone, polypropylene can be modified to prepare plastic materials with natural textures like natural stone. However, during the modification process, the appearance and mechanical properties of the plastic materials are still not comparable to those of natural stone due to the different modification methods. Therefore, the mechanical properties, scratch resistance and texture of the modified polypropylene materials are poor, and the gloss of the material is too different from that of the actual marble material, the texture is poor, and the energy consumption in the preparation process is high and the production efficiency is low, which are still technical problems that need to be solved urgently. Summary of the invention
[0009] In view of the above problems, the present invention provides a modified polyolefin material and a preparation method and use thereof. The modified polyolefin material is prepared by mixing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder with a special combined screw structure. The modified polyolefin material has clear texture, natural surface bumps, high gloss, good mechanical properties, low odor, and is green and environmentally friendly.
[0010] The invention provides a modified polyolefin material. The modified polyolefin material is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder. The modified polyolefin material has a tensile strength of 30-60MPa, a bending modulus of 2500-5000MPa, and a 23°C cantilever beam notched impact strength of 4-8kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 0.5-1.5; Taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: Polypropylene: 40-80%; Ultra-high molecular weight polyethylene: 5-15%; Mineral powder: 10-45%; Compatibilizer: 3-8%; Flash powder: 0.2-20%; Surfactant: 0.3-0.8%; Antioxidant: 0.2-0.8%; Lubricant: 0.2-0.6%; Pigment: 0.3-2%.
[0011] Furthermore, the 25°C melt index of the polypropylene is 3-100 g / 10 min.
[0012] Furthermore, the molecular weight of the ultra-high molecular weight polyethylene is 1-5 million, the mesh size is 200-800 mesh, and the diameter is 25-60 μm.
[0013] Furthermore, the mineral powder is one or more of talc, calcium carbonate, barium sulfate, silica powder, wollastonite, diatomaceous earth, attapulgite, kaolin and whiskers.
[0014] Furthermore, the compatibilizer is one or more of maleic anhydride grafted polypropylene and maleic anhydride grafted ethylene-octene copolymer.
[0015] Furthermore, the flash powder is one or more of glass fiber, glass flakes, glass beads, pearl powder, mica powder and aluminum powder.
[0016] Furthermore, the surfactant is one or more of titanate, aluminate, silane coupling agent, silicon-aluminate and borane coupling agent.
[0017] Furthermore, the silane coupling agent is one or more of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tri (β-methoxyethoxy) silane.
[0018] Furthermore, the antioxidant is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris[2,4-di-tert-butylphenyl]phosphite.
[0019] Furthermore, the lubricant is vinyl bisstearamide.
[0020] Furthermore, the pigment is one or more of titanium dioxide, carbon black and ultramarine blue.
[0021] Furthermore, the combined screw structure of the twin-screw extruder is sequentially divided into a mixing section, a kneading section, a melting section, a shearing section and an extrusion section; The mixing section includes a first conveying section, which includes conveying blocks with pitches / total lengths of 56 / 56A, 112 / 112SK, 112 / 112SK, 72 / 72, and 56 / 56 arranged in sequence; The mixing section sequentially includes a first meshing section, a second conveying section and a second meshing section, The first meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 30° / 7 / 72, 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The second conveying section includes a conveying block with a pitch / total length of 72 / 72; The second meshing section includes meshing blocks with meshing disc angle / meshing disc number / total length arranged in sequence of 45° / 5 / 56, 90° / 5 / 56, and 45° / 5 / 56; The melting section includes a third conveying section, which includes a reverse block with a pitch / total length L of 56 / 28L and a conveying block with a pitch / total length of 112 / 112SK, 112 / 112SK arranged in sequence; The shearing section includes a fourth conveying section, which includes conveying blocks with pitches / total lengths of 112 / 112SK, 112 / 112SK, and 112 / 112SK arranged in sequence; The extrusion section includes a third meshing section, a toothed disc 56, a fifth conveying section, a fourth meshing section, a sixth conveying section, a fifth meshing section, a seventh conveying section, a sixth meshing section, an eighth conveying section, a seventh meshing section, and a ninth conveying section in sequence. The third meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 45° / 5 / 56 and 60° / 4 / 56; The fifth conveying section includes a conveying block with a pitch / total length of 56 / 56; The fourth meshing section includes meshing disc angle / meshing disc number / total length arranged in sequence as 45° / 5 / 56, 60° / 4 / 56; The sixth conveying section includes conveying blocks with pitch / total length of 72 / 72, 72 / 72, and 56 / 56 arranged in sequence; The fifth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The seventh conveying section includes a conveying block with a pitch / total length of 56 / 56; The sixth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 45° / 5 / 36; The eighth conveying section includes conveying blocks with pitch / total length of 96 / 96, 96 / 96, 96 / 96 arranged in sequence; The seventh meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 90° / 5 / 56; The ninth conveying section includes a reverse block with a pitch / total length L of 56 / 28L and conveying blocks with a pitch / total length of 96 / 96, 96 / 96, 96 / 96, 72 / 72, 56 / 56, 56 / 56, 56 / 56, 56 / 56, 56 / 28, which are arranged in sequence.
[0022] The present invention also provides a method for preparing a modified polyolefin material, wherein each component is weighed according to its content, and the preparation method comprises the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, glitter powder, surfactant, antioxidant, lubricant and pigment, putting them into a high-speed mixer, stirring to obtain a mixture; Step 2: feeding the mixed material to a twin-screw extruder meshing in the same direction, melting and extruding the mixed material in the twin-screw extruder, cooling the mixed material with water at room temperature, naturally air-drying the mixed material, and pelletizing the mixed material to obtain the modified polyolefin material.
[0023] Furthermore, the mass ratio of the polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, glitter powder, surfactant, antioxidant, lubricant and pigment in step 1 is (40-80): (5-15): (10-45): (3-8): (0.2-20): (0.3-0.8): (0.2-0.8): (0.2-0.6): (0.3-2).
[0024] Furthermore, the 25°C melt index of the polypropylene in step 1 is 3-100 g / 10 min.
[0025] Furthermore, the ultra-high molecular weight polyethylene in step 1 has a molecular weight of 1-5 million, a mesh size of 200-800 meshes, and a diameter of 25-60 μm.
[0026] Furthermore, the mineral powder in step 1 is one or more of talc, calcium carbonate, barium sulfate, silica powder, wollastonite, diatomaceous earth, attapulgite, kaolin and whiskers.
[0027] Furthermore, the compatibilizer in step 1 is one or more of maleic anhydride grafted polypropylene and maleic anhydride grafted ethylene-octene copolymer.
[0028] Furthermore, the flash powder in step 1 is one or more of glass fiber, glass flakes, glass beads, pearl powder, mica powder and aluminum powder.
[0029] Furthermore, the surfactant in step 1 is one or more of titanate, aluminate, silane coupling agent, silicon-aluminate, borane coupling agent and borate coupling agent.
[0030] Furthermore, the silane coupling agent is one or more of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tri (β-methoxyethoxy) silane.
[0031] Furthermore, the antioxidant in step 1 is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and tris[2,4-di-tert-butylphenyl]phosphite.
[0032] Furthermore, the lubricant in step 1 is vinyl bisstearamide.
[0033] Furthermore, the pigment in step 1 is one or more of titanium dioxide, carbon black and ultramarine blue.
[0034] Furthermore, in step 1, the stirring speed is 500-2000 r / min, and the stirring time is 5-20 min.
[0035] Further, the operating temperature of the twin-screw extruder in the step 2 is 180-220°C, which is divided into fourteen temperature zones, wherein the first temperature zone is 180-190°C, the second temperature zone is 190-200°C, the third temperature zone is 200-210°C, the fourth temperature zone is 200-210°C, the fifth temperature zone is 210-220°C, the sixth temperature zone is 210-220°C, the seventh temperature zone is 210-220°C, the eighth temperature zone is 210-220°C, the ninth temperature zone is 210-220°C, the tenth temperature zone is 210-220°C, the eleventh temperature zone is 200-210°C, the twelfth temperature zone is 200-210°C, the thirteenth temperature zone is 190-200°C, and the fourteenth temperature zone is 190-200°C.
[0036] Furthermore, the main screw speed of the twin-screw extruder in step 2 is 200-400r / min.
[0037] Furthermore, the feeding rate of the main feeding port of the twin-screw extruder in step 2 is 100-500kg / h.
[0038] Furthermore, the twin-screw extruder in step 2 can also be fed through a side feeding port, and the feeding amount of the side feeding port is 30-50kg / h.
[0039] Furthermore, when the flash powder is glass fiber and / or glass flake and / or glass microbead and / or mica, the glass fiber and / or glass flake and / or glass microbead and / or mica are fed through the main feeding port or the side feeding port of the twin-screw extruder.
[0040] Furthermore, the aspect ratio of the twin-screw extruder in step 2 is (30-60):1.
[0041] Furthermore, the pelletized particles in step 2 are cylindrical with a length of 3-5 mm and a diameter of 2.5-4 mm.
[0042] Furthermore, the combined screw of the twin-screw extruder in step 2 is sequentially divided into a mixing section, a kneading section, a venting section, a side feeding section and an extrusion section; The mixing section includes a first conveying section, which includes conveying blocks with pitches / total lengths of 56 / 56A, 112 / 112SK, 112 / 112SK, 72 / 72, and 56 / 56 arranged in sequence; The mixing section sequentially includes a first meshing section, a second conveying section and a second meshing section, The first meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 30° / 7 / 72, 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The second conveying section includes a conveying block with a pitch / total length of 72 / 72; The second meshing section includes meshing blocks with meshing disc angle / meshing disc number / total length arranged in sequence of 45° / 5 / 56, 90° / 5 / 56, and 45° / 5 / 56; The melting section includes a third conveying section, which includes a reverse block with a pitch / total length L of 56 / 28L and a conveying block with a pitch / total length of 112 / 112SK, 112 / 112SK arranged in sequence; The shearing section includes a fourth conveying section, which includes conveying blocks with pitches / total lengths of 112 / 112SK, 112 / 112SK, and 112 / 112SK arranged in sequence; The extrusion section includes a third meshing section, a toothed disc 56, a fifth conveying section, a fourth meshing section, a sixth conveying section, a fifth meshing section, a seventh conveying section, a sixth meshing section, an eighth conveying section, a seventh meshing section, and a ninth conveying section in sequence. The third meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 45° / 5 / 56 and 60° / 4 / 56; The fifth conveying section includes a conveying block with a pitch / total length of 56 / 56; The fourth meshing section includes meshing disc angle / meshing disc number / total length arranged in sequence as 45° / 5 / 56, 60° / 4 / 56; The sixth conveying section includes conveying blocks with pitch / total length of 72 / 72, 72 / 72, and 56 / 56 arranged in sequence; The fifth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The seventh conveying section includes a conveying block with a pitch / total length of 56 / 56; The sixth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 45° / 5 / 36; The eighth conveying section includes conveying blocks with pitch / total length of 96 / 96, 96 / 96, 96 / 96 arranged in sequence; The seventh meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 90° / 5 / 56; The ninth conveying section includes a reverse block with a pitch / total length L of 56 / 28L and conveying blocks with a pitch / total length of 96 / 96, 96 / 96, 96 / 96, 72 / 72, 56 / 56, 56 / 56, 56 / 56, 56 / 56, 56 / 28, which are arranged in sequence.
[0043] Furthermore, the main feeding port corresponds to the first temperature zone of the twin-screw extruder.
[0044] Furthermore, the side feeding port corresponds to the sixth temperature zone, the seventh temperature zone, or the eighth temperature zone of the twin-screw extruder.
[0045] A use of the modified polyolefin material, wherein the modified polyolefin material is used for preparing imitation clay, imitation marble and imitation natural soil and stone materials.
[0046] Beneficial effects of the present invention: 1. The present invention blends polypropylene and ultra-high molecular weight polyethylene. Since the ultra-high molecular weight polyethylene is in the form of powder or small particles, which is different from polypropylene, during the blending process, the ultra-high molecular weight polyethylene is wrapped by polypropylene and embedded in the polypropylene resin without being obviously stretched, so that the surface of the material is uneven, thereby increasing the diffuse reflection effect and reducing the glossiness. At the same time, the ultra-high molecular weight polyethylene is spherical, and the sphere has a roller effect, which can effectively disperse stress and reduce surface damage, thereby improving the scratch resistance of the material. In addition, since the ultra-high molecular weight polyethylene has a large molecular weight and a high degree of polymerization, it has good dispersibility when mixed with materials such as polypropylene, and no precipitation will occur after long-term use. At the same time, the content of ultra-high molecular weight polyethylene in the present invention is moderate, and the compatibility will not be affected by excessive content of ultra-high molecular weight polyethylene; 2. The present invention adds mineral powder and flash powder, wherein the mineral powder enhances the strength of polypropylene and increases the weight of the material, making the material more in line with the texture of imitation soil and stone materials; and the addition of flash powder provides a small amount of flash points for the material, so that the material can achieve a multi-level appearance effect, but the mineral powder and flash powder are inorganic materials, and in the process of blending with organic substances such as polypropylene, they will be difficult to mix due to compatibility. Therefore, the present invention also adds a compatibilizer and a surfactant, wherein the compatibilizer contains maleic anhydride and double bonds, which can improve the compatibility of inorganic materials and organic materials, improve the tensile and impact strength of the product, achieve high filling, reduce the amount of resin, improve processing rheology, and improve surface finish; and the molecular chain of the surfactant is relatively soft, and can be bent and entangled with the organic polymer, so that the compatibility of organic and inorganic substances is improved, and the impact strength of the material is improved. At the same time, after the scratch resistance test, the surface of the modified polyolefin material described in the present invention can still maintain its original state, the marks are not obvious, and the scratch resistance is good; 3. The present invention also blends the materials through a specific twin-screw extruder, wherein a toothed disk 56 is provided in the extrusion section of the combined screw structure to shear the molten material, thereby reducing energy consumption during processing and making the material more dispersible in the twin-screw extruder. At the same time, due to the addition of lubricant, the friction of the material during the extrusion process of the twin-screw extruder is reduced, thereby reducing energy consumption and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 It is a combined screw structure diagram of the co-rotating meshing twin-screw extruder described in Examples 1-9 and Comparative Examples 1-4 of the present invention; Figure 2 This is a scanning electron microscope image of the modified polyolefin material described in Example 1 magnified 56 times; Figure 3 This is a scanning electron microscope image of the modified polyolefin material described in Example 1 magnified 150 times; Figure 4 This is a scanning electron microscope image of the modified polyolefin material described in Example 6 magnified 150 times; Figure 5 This is a scanning electron microscope image of the modified polyolefin material described in Example 7 magnified 150 times; Figure 6 is a scanning electron microscope image of the modified polyolefin materials described in Examples 2, 5, 7 and 8 after the scratch resistance test; Figure 7 This is a scanning electron microscope image of the modified polyolefin materials described in Comparative Examples 3 and 4 after the scratch resistance test. DETAILED DESCRIPTION
[0048] The invention is described in detail below with reference to the embodiments: The invention provides a modified polyolefin material and a preparation method and use thereof. The modified polyolefin material has good mechanical properties and scratch resistance, and at the same time has a very high imitation soil and stone effect. The surface of the material has the micro-shimmer effect and the texture and feel of soil and stone materials, and the stability is greatly improved.
[0049] Example 1 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 37MPa, a flexural modulus of 3600MPa, and a 23°C cantilever beam notched impact strength of 7kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.3.
[0050] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 55.3%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% 200-mesh glass flakes and 0.2% pearlescent; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0051] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a co-rotating twin-screw extruder, feed the glass flakes from the side feeding port of the co-rotating twin-screw extruder, melt-extrude in the twin-screw extruder, water-cool at room temperature, naturally air-dry, and pelletize to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0052] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0053] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, clay-like appearance.
[0054] like Figure 2 This is a scanning electron microscope image of the modified polyolefin material described in Example 1 magnified 56 times. It can be seen from the image that the glass flakes are evenly dispersed in the material and the texture of the material is good.
[0055] like Figure 3 This is a scanning electron microscope image of the modified polyolefin material described in Example 1 magnified 150 times. It can be seen from the image that the structure of the glass flakes in the image is clear, and due to the addition of pearlescent light to the material, a clear slight flash can also be seen in the material.
[0056] Example 2 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 35MPa, a flexural modulus of 3500MPa, and a 23°C cantilever beam notched impact strength of 6.8kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.4.
[0057] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 55.5%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The flash powder is 10% 200 mesh glass flakes; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0058] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a co-rotating twin-screw extruder, feed the glass flakes from the side feeding port of the co-rotating twin-screw extruder, melt-extrude in the twin-screw extruder, water-cool at room temperature, naturally air-dry, and pelletize to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0059] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0060] The surface of the modified polyolefin material obtained in this embodiment presents a matte, fine-textured, clay-like appearance.
[0061] Example 3 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 55MPa, a flexural modulus of 4500MPa, and a 23°C cantilever beam notched impact strength of 7.5kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.
[0062] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 55.3%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% glass fiber and 0.2% pearl; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0063] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixed material from the main feeding port of a co-rotating twin-screw extruder, feed the glass fiber from the side feeding port of the co-rotating twin-screw extruder, melt-extrude the mixed material in the twin-screw extruder, cool the mixed material with water at room temperature, air-dry the mixed material naturally, and pelletize the mixed material to obtain the modified polyolefin material having a length of 3 mm and a diameter of 2.5 mm.
[0064] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0065] The surface of the modified polyolefin material obtained in this example presents an apparent shiny, fine-textured marble-like appearance.
[0066] Example 4 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 50MPa, a flexural modulus of 4000MPa, and a 23°C cantilever beam notched impact strength of 6.5kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.2.
[0067] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 55.3%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh size is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% glass fiber and 0.2% pearl; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0068] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, glass fiber, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a twin-screw extruder meshing in the same direction, melt and extrude it in the twin-screw extruder, water-cool it at room temperature, naturally air-dry it, and pelletize it to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0069] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 450kg / h, and the aspect ratio is 40:1.
[0070] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, fine-textured marble-like appearance.
[0071] Example 5 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 35MPa, a flexural modulus of 2900MPa, and a 23°C cantilever beam notched impact strength of 4kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.5.
[0072] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 57.5%, and the polypropylene has a melting index of 25 g / 10 min at 25°C; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% mica powder and 1.0% pearlescent; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0073] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixed material from the main feeding port of a co-rotating twin-screw extruder, feed the mica from the side feeding port of the co-rotating twin-screw extruder, melt-extrude in the twin-screw extruder, water-cool at room temperature, naturally air-dry, and pelletize to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0074] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0075] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, matte, fine-textured clay-like appearance.
[0076] Example 6 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 39MPa, a flexural modulus of 3650MPa, and a 23°C cantilever beam notched impact strength of 6.7kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.1.
[0077] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 60.6%, and the polypropylene has a melting index of 25 g / 10 min at 25°C; The ultra-high molecular weight polyethylene is 5%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% 200-mesh glass flakes and 0.2% pearlescent; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0078] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a co-rotating twin-screw extruder, feed the glass flakes from the side feeding port of the co-rotating twin-screw extruder, melt-extrude in the twin-screw extruder, water-cool at room temperature, naturally air-dry, and pelletize to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0079] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0080] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, fine-textured, stone-like appearance.
[0081] like Figure 4 This is a scanning electron microscope image of the modified polyolefin material described in Example 6 magnified 150 times. The glass flakes in the image are well dispersed and have obvious pearlescence.
[0082] Example 7 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 35MPa, a flexural modulus of 3700MPa, and a 23°C cantilever beam notched impact strength of 7.4kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.
[0083] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 50.3%, and the polypropylene has a melting index of 25 g / 10 min at 25°C; The ultra-high molecular weight polyethylene is 15%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% 200-mesh glass flakes and 0.2% pearlescent; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0084] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a co-rotating twin-screw extruder, feed the glass flakes from the side feeding port of the co-rotating twin-screw extruder, melt-extrude in the twin-screw extruder, water-cool at room temperature, naturally air-dry, and pelletize to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0085] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0086] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, coarse-textured, stone-like appearance.
[0087] like Figure 5 This is a scanning electron microscope image of the modified polyolefin material described in Example 7 at 150 times magnification. In the image, glass flakes are stably present in the material and have good dispersion.
[0088] Example 8 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 33MPa, a flexural modulus of 2720MPa, and a 23°C cantilever beam notched impact strength of 4.5kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.4.
[0089] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 57.8%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh size is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talc and 10% barium sulfate; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 0.5% pearlescent; The surfactant is 0.6% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0090] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a twin-screw extruder meshing in the same direction, melt and extrude it in the twin-screw extruder, water-cool it at room temperature, naturally air-dry it, and pelletize it to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0091] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 450kg / h, and the aspect ratio is 40:1.
[0092] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, fine-textured clay-like appearance.
[0093] like Figure 6 The scanning electron microscope images of the modified polyolefin materials described in Examples 2, 5, 7 and 8 after the scratch resistance test show that the materials in the images have slight marks after the scratch resistance test, and there is no large-scale wear on the surface of the materials, only shallow scratches.
[0094] Example 9 The present embodiment provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 45MPa, a flexural modulus of 3500MPa, and a 23°C cantilever beam notched impact strength of 7.5kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.2.
[0095] In this embodiment, taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 57.8%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh number is 200 mesh, and the diameter is 30 μm; The mineral powder is 10% talc and 10% barium sulfate; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% glass fiber and 0.5% pearl; The surfactant is 0.6% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0096] This embodiment provides a method for preparing a modified polyolefin material. The components are weighed according to their contents. The preparation method includes the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a twin-screw extruder meshing in the same direction, melt and extrude it in the twin-screw extruder, water-cool it at room temperature, naturally air-dry it, and pelletize it to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0097] The working temperature of the twin-screw extruder described in this embodiment is 190-220°C, and it is evenly divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 450kg / h, and the aspect ratio is 40:1.
[0098] The surface of the modified polyolefin material obtained in this example presents a slightly shiny, fine-textured, stone-like appearance.
[0099] Comparative Example 1 The comparative example provides a modified polyolefin material, which is prepared by blending polypropylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 39MPa, a flexural modulus of 3580MPa, and a 23°C cantilever beam notched impact strength of 6.7kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.6.
[0100] In this comparative example, taking the total mass of each component in the modified polyolefin material as 100% as the benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 65.3%, and the polypropylene has a melt index of 25 g / 10 min at 25°C; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% 200-mesh glass flakes and 0.2% pearlescent; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0101] This comparative example provides a method for preparing a modified polyolefin material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, weigh polypropylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment, put them into a high-speed mixer, and stir them at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a co-rotating twin-screw extruder, feed the glass flakes from the side feeding port of the co-rotating twin-screw extruder, melt-extrude in the twin-screw extruder, water-cool at room temperature, naturally air-dry, and pelletize to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0102] The working temperature of the twin-screw extruder in this comparative example is 190-220°C, and it is divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0103] The surface of the modified polyolefin material obtained in this comparative example presents a slightly glittering appearance.
[0104] Comparative Example 2 The comparative example provides a modified polyolefin material, which is prepared by blending polypropylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 59MPa, a flexural modulus of 4560MPa, and a 23°C cantilever beam notched impact strength of 7kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.4.
[0105] In this comparative example, taking the total mass of each component in the modified polyolefin material as 100% as the benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 65.3%, and the polypropylene has a melt index of 25 g / 10 min at 25°C; The mineral powder is 20% talcum powder; The compatibilizer is 3% maleic anhydride grafted polypropylene; The glitter powder is 10% glass fiber and 0.2% pearl; The surfactant is 0.4% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0106] This comparative example provides a method for preparing a modified polyolefin material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, weigh polypropylene, mineral powder, compatibilizer, pearlescent agent, surfactant, antioxidant, lubricant and pigment, put them into a high-speed mixer, and stir them at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixed material from the main feeding port of a co-rotating twin-screw extruder, feed the glass fiber from the side feeding port of the co-rotating twin-screw extruder, melt-extrude the mixed material in the twin-screw extruder, cool the mixed material with water at room temperature, air-dry the mixed material naturally, and pelletize the mixed material to obtain the modified polyolefin material having a length of 3 mm and a diameter of 2.5 mm.
[0107] The working temperature of the twin-screw extruder in this comparative example is 190-220°C, and it is divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 400kg / h, the feeding amount of the side feeding port is 44.5kg / h, and the aspect ratio is 40:1.
[0108] The surface of the modified polyolefin material obtained in this comparative example presents an obvious shiny appearance.
[0109] Comparative Example 3 The comparative example provides a modified polyolefin material, which is prepared by blending polypropylene, mineral powder, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 34MPa, a flexural modulus of 3200MPa, and a 23°C cantilever beam notched impact strength of 4kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 2.1.
[0110] In this comparative example, taking the total mass of each component in the modified polyolefin material as 100% as the benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 68.1%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The mineral powder is 20% talc and 10% barium sulfate; The glitter powder is 0.2% pearlescent; The surfactant is 0.6% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0111] This comparative example provides a method for preparing a modified polyolefin material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, weigh polypropylene, mineral powder, pearlescent agent, surfactant, antioxidant, lubricant and pigment, put them into a high-speed mixer, and stir them at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a twin-screw extruder meshing in the same direction, melt and extrude it in the twin-screw extruder, water-cool it at room temperature, naturally air-dry it, and pelletize it to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0112] The working temperature of the twin-screw extruder in this comparative example is 190-220°C, and it is divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 450kg / h, and the aspect ratio is 40:1.
[0113] The surface of the modified polyolefin material obtained in this comparative example presents a slightly shiny matte appearance.
[0114] Comparative Example 4 The comparative example provides a modified polyolefin material, which is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 32MPa, a flexural modulus of 2850MPa, and a 23°C cantilever beam notched impact strength of 4.6kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 1.8.
[0115] In this comparative example, taking the total mass of each component in the modified polyolefin material as 100% as the benchmark, the components and the content of each component in the modified polyolefin material are: The polypropylene is 58.3%, and the polypropylene has a 25°C melt index of 25 g / 10 min; The ultra-high molecular weight polyethylene is 10%, the molecular weight of the ultra-high molecular weight polyethylene is 2 million, the mesh size is 200 mesh, and the diameter is 30 μm; The mineral powder is 20% talc and 10% barium sulfate; The surfactant is 0.6% borane coupling agent; The antioxidants are 0.1% pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and 0.2% tris[2,4-di-tert-butylphenyl]phosphite; The lubricant is 0.5% vinyl bisstearamide; The pigment is 0.3% carbon black.
[0116] This comparative example provides a method for preparing a modified polyolefin material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, surfactant, antioxidant, lubricant and pigment, putting them into a high-speed mixer, stirring at a speed of 1000 r / min for 10 minutes to obtain a mixture; Step 2: Feed the mixture from the main feeding port of a twin-screw extruder meshing in the same direction, melt and extrude it in the twin-screw extruder, water-cool it at room temperature, naturally air-dry it, and pelletize it to obtain the modified polyolefin material with a length of 3 mm and a diameter of 2.5 mm.
[0117] The working temperature of the twin-screw extruder in this comparative example is 190-220°C, and it is divided into fourteen temperature zones according to the screw length, wherein the first temperature zone is 190°C, the second temperature zone is 200°C, the third temperature zone is 210°C, the fourth temperature zone is 210°C, the fifth temperature zone is 220°C, the sixth temperature zone is 220°C, the seventh temperature zone is 220°C, the eighth temperature zone is 220°C, the ninth temperature zone is 220°C, the tenth temperature zone is 220°C, the eleventh temperature zone is 210°C, the twelfth temperature zone is 210°C, the thirteenth temperature zone is 200°C, and the fourteenth temperature zone is 200°C; the main screw speed of the twin-screw extruder is 350r / min, the feeding amount of the main feeding port is 450kg / h, and the aspect ratio is 40:1.
[0118] The surface of the modified polyolefin material obtained in this comparative example presents a non-glittering appearance.
[0119] like Figure 7 The scanning electron microscope images of the modified polyolefin materials described in Comparative Examples 3 and 4 after the scratch resistance test show that the materials in the images have pit-like wear on the surface after the scratch resistance test, and the degree of wear is large.
[0120] The scratch resistance test conditions in the present invention are 10N and 1000mm / min.
[0121] like Figure 1 The combined screw structure diagram of the co-rotating meshing twin-screw extruder described in Examples 1-9 and Comparative Examples 1-4 of the present invention is sequentially divided into a mixing section, a kneading section, a melting section, a shearing section and an extrusion section; The mixing section includes a first conveying section, which includes conveying blocks with pitches / total lengths of 56 / 56A, 112 / 112SK, 112 / 112SK, 72 / 72, and 56 / 56 arranged in sequence; The mixing section sequentially includes a first meshing section, a second conveying section and a second meshing section, The first meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 30° / 7 / 72, 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The second conveying section includes a conveying block with a pitch / total length of 72 / 72; The second meshing section includes meshing blocks with meshing disc angle / meshing disc number / total length arranged in sequence of 45° / 5 / 56, 90° / 5 / 56, and 45° / 5 / 56; The melting section includes a third conveying section, which includes a reverse block with a pitch / total length L of 56 / 28L and a conveying block with a pitch / total length of 112 / 112SK, 112 / 112SK arranged in sequence; The shearing section includes a fourth conveying section, which includes conveying blocks with pitches / total lengths of 112 / 112SK, 112 / 112SK, and 112 / 112SK arranged in sequence; The extrusion section includes a third meshing section, a toothed disc 56, a fifth conveying section, a fourth meshing section, a sixth conveying section, a fifth meshing section, a seventh conveying section, a sixth meshing section, an eighth conveying section, a seventh meshing section, and a ninth conveying section in sequence. The third meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 45° / 5 / 56 and 60° / 4 / 56; The fifth conveying section includes a conveying block with a pitch / total length of 56 / 56; The fourth meshing section includes meshing disc angle / meshing disc number / total length arranged in sequence as 45° / 5 / 56, 60° / 4 / 56; The sixth conveying section includes conveying blocks with pitch / total length of 72 / 72, 72 / 72, and 56 / 56 arranged in sequence; The fifth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The seventh conveying section includes a conveying block with a pitch / total length of 56 / 56; The sixth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 45° / 5 / 36; The eighth conveying section includes conveying blocks with pitch / total length of 96 / 96, 96 / 96, 96 / 96 arranged in sequence; The seventh meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 90° / 5 / 56; The ninth conveying section includes a reverse block with a pitch / total length L of 56 / 28L and conveying blocks with a pitch / total length of 96 / 96, 96 / 96, 96 / 96, 72 / 72, 56 / 56, 56 / 56, 56 / 56, 56 / 56, 28 / 56, which are arranged in sequence.
[0122] The manufacturer of the borane coupling agent in the present invention is Qingdao Siwei Chemical Industry, and the brand is SB-181.
[0123] Table 1 shows the components and their contents in Examples 1-9 and Comparative Examples 1-4.
[0124] The antioxidant 1010 described in Table 1 is pentaerythritol tetrakis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate, and the antioxidant 168 is tris(2,4-di-tert-butylphenyl) phosphite.
[0125] Table 2 shows the material properties of Examples 1-9 and Comparative Examples 1-4
[0126] As shown in Tables 1 and 2, in Examples 1-7, different types and contents of the added flash powder can be used to prepare modified polyolefin materials with different appearance effects. In Examples 8-9, different types and contents of the added mineral powder are used, and the obtained modified polyolefin materials have stable mechanical properties and can still achieve the appearance effect of imitating marble or clay. The glass fibers in Examples 4 and 9 are fed from the main feeding port of the twin-screw extruder, and the glass fibers are sheared in the twin-screw extruder for better dispersion. The obtained modified polyolefin materials can achieve different appearance effects. In Comparative Examples 1 and 2, no ultra-high molecular weight polyethylene is added, and the prepared materials do not have a texture effect, have a poor texture, and cannot achieve the effect of imitating marble and clay. Comparative Examples 3 and 4 do not add compatibilizers and flash powder, which greatly reduces the mechanical properties of the materials and loses the texture and flash effects of imitating marble and clay. When ultra-high molecular weight polyethylene is added without adding pearlescent, the texture effect can be achieved, but the three-dimensional micro-shimmering marble effect cannot be achieved.
[0127] In the present invention, the scratch resistance ΔL is the value L2 after scratching minus the value L1 before scratching measured by a colorimeter when the material is subjected to a scratch resistance test using a cross scratch tester.
[0128] Based on the above, it can be seen that the modified polyolefin material described in this patent has a wide range of applications, low cost, and extremely high market prospects.
[0129] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
Claims
1. A modified polyolefin material, characterized in that: The modified polyolefin material is prepared by blending polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, flash powder, surfactant, antioxidant, lubricant and pigment in a twin-screw extruder; the modified polyolefin material has a tensile strength of 30-60MPa, a flexural modulus of 2500-5000MPa, and a 23°C cantilever beam notched impact strength of 4-8kJ / m 2 ; The scratch resistance ΔL of the modified polyolefin material is 0.5-1.5; Taking the total mass of each component in the modified polyolefin material as 100% as a benchmark, the components and the content of each component in the modified polyolefin material are: Polypropylene: 40-80%; Ultra-high molecular weight polyethylene: 5-15%; Mineral powder: 10-45%; Compatibilizer: 3-8%; Flash powder: 0.2-20%; Surfactant: 0.3-0.8%; Antioxidant: 0.2-0.8% Lubricant: 0.2-0.6%; Pigment: 0.3-2%.
2. The modified polyolefin material according to claim 1, characterized in that: The ultra-high molecular weight polyethylene has a molecular weight of 1-5 million, a mesh size of 200-800 meshes, and a diameter of 25-60 μm.
3. The modified polyolefin material according to claim 1, characterized in that: The flash powder is one or more of glass fiber, glass flakes, glass microbeads, pearl powder, mica powder and aluminum powder.
4. The modified polyolefin material according to claim 1, characterized in that: The combined screw structure of the twin-screw extruder is sequentially divided into a mixing section, a kneading section, a melting section, a shearing section and an extrusion section; The mixing section includes a first conveying section, which includes conveying blocks with pitches / total lengths of 56 / 56A, 112 / 112SK, 112 / 112SK, 72 / 72, and 56 / 56 arranged in sequence; The mixing section sequentially includes a first meshing section, a second conveying section and a second meshing section, The first meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 30° / 7 / 72, 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The second conveying section includes a conveying block with a pitch / total length of 72 / 72; The second meshing section includes meshing blocks with meshing disc angle / meshing disc number / total length arranged in sequence of 45° / 5 / 56, 90° / 5 / 56, and 45° / 5 / 56; The melting section includes a third conveying section, which includes a reverse block with a pitch / total length L of 56 / 28L and a conveying block with a pitch / total length of 112 / 112SK, 112 / 112SK arranged in sequence; The shearing section includes a fourth conveying section, which includes conveying blocks with pitches / total lengths of 112 / 112SK, 112 / 112SK, and 112 / 112SK arranged in sequence; The extrusion section includes a third meshing section, a toothed disc 56, a fifth conveying section, a fourth meshing section, a sixth conveying section, a fifth meshing section, a seventh conveying section, a sixth meshing section, an eighth conveying section, a seventh meshing section, and a ninth conveying section in sequence. The third meshing section includes meshing blocks with meshing disc angle / number of meshing discs / total length arranged in sequence of 45° / 5 / 56 and 60° / 4 / 56; The fifth conveying section includes a conveying block with a pitch / total length of 56 / 56; The fourth meshing section includes meshing disc angle / meshing disc number / total length arranged in sequence as 45° / 5 / 56, 60° / 4 / 56; The sixth conveying section includes conveying blocks with pitch / total length of 72 / 72, 72 / 72, and 56 / 56 arranged in sequence; The fifth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 60° / 4 / 56; The seventh conveying section includes a conveying block with a pitch / total length of 56 / 56; The sixth meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 45° / 5 / 36; The eighth conveying section includes conveying blocks with pitch / total length of 96 / 96, 96 / 96, 96 / 96 arranged in sequence; The seventh meshing section includes meshing blocks whose meshing disc angle / number of meshing discs / total length are arranged in sequence as 45° / 5 / 56, 45° / 5 / 56, and 90° / 5 / 56; The ninth conveying section includes a reverse block with a pitch / total length L of 56 / 28L and conveying blocks with a pitch / total length of 96 / 96, 96 / 96, 96 / 96, 72 / 72, 56 / 56, 56 / 56, 56 / 56, 56 / 56, 56 / 28, which are arranged in sequence.
5. A method for preparing the modified polyolefin material according to any one of claims 1 to 4, characterized in that: Weigh each component according to its content, and the preparation method comprises the following steps: Step 1, weighing polypropylene, ultra-high molecular weight polyethylene, mineral powder, compatibilizer, glitter powder, surfactant, antioxidant, lubricant and pigment, putting them into a high-speed mixer, stirring to obtain a mixture; Step 2: feeding the mixed material to a twin-screw extruder meshing in the same direction, melting and extruding the mixed material in the twin-screw extruder, cooling the mixed material with water at room temperature, naturally air-drying the mixed material, and pelletizing the mixed material to obtain the modified polyolefin material.
6. The preparation method according to claim 5, characterized in that: The working temperature of the twin-screw extruder in the step 2 is 180-220°C, which is divided into fourteen temperature zones, wherein the first temperature zone is 180-190°C, the second temperature zone is 190-200°C, the third temperature zone is 200-210°C, the fourth temperature zone is 200-210°C, the fifth temperature zone is 210-220°C, the sixth temperature zone is 210-220°C, the seventh temperature zone is 210-220°C, the eighth temperature zone is 210-220°C, the ninth temperature zone is 210-220°C, the tenth temperature zone is 210-220°C, the eleventh temperature zone is 200-210°C, the twelfth temperature zone is 200-210°C, the thirteenth temperature zone is 190-200°C, and the fourteenth temperature zone is 190-200°C.
7. The preparation method according to claim 5, characterized in that: The feeding rate of the main feeding port of the twin-screw extruder in step 2 is 100-500kg / h.
8. The preparation method according to claim 5, characterized in that: The twin-screw extruder in step 2 can also be fed through a side feeding port, and the feeding amount of the side feeding port is 30-50kg / h.
9. The preparation method according to claim 5, characterized in that: The aspect ratio of the twin-screw extruder in step 2 is (30-60):
1.
10. Use of the modified polyolefin material according to any one of claims 1 to 4, characterized in that: The modified polyolefin material is used for preparing imitation clay, imitation marble and imitation natural soil and stone materials.
Citation Information
Cited By
Scratch-proof polypropylene film for packaging and preparation process thereof
CN120056550A