Mesenchymal stem cell scaffold as well as preparation method and application thereof

Through mesenchymal stem cells and scaffolds of degradable biological materials, 3D printing technology is used to form a gradient-distributed cell scaffold, which solves the complex problems of vascular reperfusion injury and nanoparticle preparation in the prior art, and achieves continuous in the ischemic site Angiogenesis and microenvironment improve, reducing treatment costs.

CN119040257APending Publication Date: 2024-11-29SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196071.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art has problems such as vascular reperfusion injury, complex nanoparticle preparation steps, high material price, and limited embedding efficiency when inducing angiogenesis, which limits the application of the treatment of ischemic diseases.

Method used

Scaffolds prepared by mesenchymal stem cells and degradable biological materials are used to form uniform or gradient-distributed cell scaffolds through 3D printing technology, and the cytokine gradient is used to promote angiogenesis, and the stability of the scaffold is improved through cross-linking technology of degradable materials.

Benefits of technology

Continuous induction of angiogenesis and extension in the ischemic site, reducing fibrosis, improving the microenvironment and vascular repair effects, and reducing treatment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040257A_ABST
    Figure CN119040257A_ABST
Patent Text Reader

Abstract

The invention discloses a mesenchymal stem cell scaffold for inducing angiogenesis, which comprises mesenchymal stem cells and a scaffold material, wherein the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed, or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increased from the periphery of the scaffold to the center of the scaffold, or is gradually increased from one end of the scaffold to the other end of the scaffold. The mesenchymal stem cell scaffold can well promote angiogenesis and extension, can be applied to heart and limb ischemia and hypoxia parts to induce angiogenesis, and has the prospects of improving microcirculation, supplying blood and oxygen and relieving and treating ischemia and hypoxia diseases.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of application number 202210313686.4, application date March 28, 2022, and invention name “Mesenchymal stem cell scaffold for inducing angiogenesis, preparation method and application thereof”. Technical Field

[0002] The present invention relates to the technical field of cell culture, and in particular to a mesenchymal stem cell scaffold for inducing angiogenesis, and a preparation method and application thereof. Background Art

[0003] At present, the reduction or interruption of blood flow caused by local vascular spasm or blockage often leads to necrosis of tissue cells in the area due to hypoxia and insufficient supply of nutrients. Continuous cell death leads to inflammation and fibrosis. The resulting cardiovascular and cerebrovascular diseases and limb ischemic diseases have high mortality and disability rates in clinical practice. Traditional treatment methods are mainly to dredge blood vessels, but the damage caused by vascular reperfusion cannot be ignored. In recent years, inducing angiogenesis in ischemic sites has become a new treatment method. Angiogenesis and maturation is a multi-factor highly temporally regulated process. The formation of new blood vessels is initiated by pro-angiogenic factors such as VEGF and bFGF, recruiting smooth muscle cells and peripheral cells pericytes, and then PDGF promotes the maturation of new blood vessels (Luís Henrique WolffGowdak and JoséEduardo Krieger, 2018). Introducing angiogenesis inducing factors such as VEGF, bFGF, PDGF, etc. in the ischemic site can induce the proliferation and migration of endothelial cells of the original blood vessels to form new blood vessels. Therefore, efficiently and conveniently introducing factors that promote angiogenesis and maturation into ischemic sites is the key to improving and treating ischemic diseases.

[0004] In current research, most of the biomacromolecules such as PLGA [poly (lactic-co-glycolic acid)] (Mohandas et al., 2015), PLLA [poly (L-lactic acid)] and fibrin (Golub et al., 2010), silk fibroin (Wang et al., 2017), and heat shock protein (Takagishi et al., 2021) are used to encapsulate cytokines such as VEGF and PDGF to make nanoparticles (NPs). The nanoparticles are then loaded into scaffold materials such as cellulose, chitin-hyaluronic acid, and hydrogels for transplantation to achieve in situ delivery and sustained and controlled release of the factors, thereby inducing angiogenesis. The loading efficiency of VEGF using bacterial cellulose / gelatin sponge is 66.5%, and more than 91% of VEGF is released within 2 days; VEGF is first made into nanoparticles with silk protein and then combined with bacterial cellulose / gelatin sponge to load almost all factors, and the sudden release of factors is significantly improved. Only 9.9% of VEGF is released on the first day, and the cumulative release rate at 28 days is 51.4% (Wang et al., 2017). The core-shell scaffold (polycaprolactone & 1% PEG) prepared by electrospinning is loaded with VEGF, and the cumulative release is 38% within 18 hours, and then reaches a plateau and slowly releases (Zigdon-Giladi et al., 2017). NPs can be prepared according to different types of cytokines as needed, among which core-shell 2-layer NPs can achieve delayed release of cytokines. For example, PLGA single-layer NPs encapsulate VEGF and bFGF, and PLGA-PLLA core-shell two-layer NPs encapsulate PDGF, which can achieve the release of VEGF and bFGF first and the delayed release of PDGF, effectively promoting angiogenesis and maturation (Izadifar et al., 2016). However, the preparation of nanoparticles has many steps and complex processes, and often requires some special instruments and equipment, such as ultrasonic material emulsification dispersers, ultra-speed refrigerated centrifuges, freeze dryers, etc. The preparation and process control of NPs involving multiple cytokines are more complicated; in addition, cytokines and encapsulation materials such as PLGA are expensive, have limited encapsulation efficiency, and have high drug preparation costs, which greatly limits their promotion and application.

[0005] In addition to using cytokines to induce the formation of new blood vessels in ischemic areas, stem cell transplantation, which then differentiates stem cells into endothelial cells and smooth muscle cells to form new blood vessels, provides a new treatment method. Embryonic stem cells, induced pluripotent stem cells, and mesenchymal stem cells all have the potential to differentiate into endothelial cells and smooth muscle cells and form new blood vessels. Among them, mesenchymal stem cells have become one of the transplant cell sources that have received much attention and recognition in clinical practice due to their wide sources, easy isolation and acquisition, strong proliferation and differentiation capabilities, low immunogenicity, and strong immune regulation and fibrosis reduction effects.

[0006] Mesenchymal stem cells not only have the potential to differentiate into new blood vessels, but also have strong paracrine ability, and can secrete water-soluble cytokines (such as vascular endothelial cell growth factor VEGF, platelet-derived growth factor PDGF, basic fibroblast growth factor bFGF, hepatocyte growth factor HGF, insulin-like growth factor IGF-1, etc.), microRNAs and exosomes, etc. These substances are considered to be important components for the therapeutic effect of mesenchymal stem cell transplantation. Among them, soluble cytokines such as VEGF, bFGF, PDGF, and HGF have the effect of inducing angiogenesis and maturation. The secretions of mesenchymal stem cells (MSCs) also have the effect of regulating immune response and reducing fibrosis, which helps to improve the microenvironment and further promote the formation and growth of new blood vessel networks. Summary of the invention

[0007] Based on this, the present invention provides a mesenchymal stem cell scaffold for inducing angiogenesis, which comprises mesenchymal stem cells and a scaffold material, wherein the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increasing from the periphery of the scaffold to the center of the scaffold, or is gradually increasing from one end of the scaffold to the other end of the scaffold.

[0008] Furthermore, the mesenchymal stem cells are selected from one or more of the following: bone marrow mesenchymal stem cells, peripheral blood mesenchymal stem cells, adipose mesenchymal stem cells, umbilical cord mesenchymal stem cells, umbilical cord blood mesenchymal stem cells, amniotic fluid mesenchymal stem cells, tooth mesenchymal stem cells, testicular mesenchymal stem cells, skin mesenchymal stem cells and placental mesenchymal stem cells.

[0009] Furthermore, the mesenchymal stem cells are autologous mesenchymal stem cells and / or allogeneic mesenchymal stem cells.

[0010] Furthermore, the autologous source is autologous peripheral blood and / or fat.

[0011] Furthermore, the allogeneic source is allogeneic umbilical cord Wharton's jelly, umbilical cord blood, amniotic fluid and / or placenta.

[0012] Furthermore, the mesenchymal stem cells secrete one or more substances selected from the following: soluble cytokines, microRNAs and exosomes.

[0013] Furthermore, the soluble cytokine is selected from one or more of the following: vascular endothelial growth factor, platelet-derived growth factor, basic fibroblast growth factor, hepatocyte growth factor, stromal cell-derived factor and insulin-like growth factor.

[0014] Furthermore, the scaffold material is a degradable biomaterial.

[0015] Further, the scaffold material is a partially degraded, modified compound such as a thermosensitive compound and / or a photosensitive compound.

[0016] Furthermore, the scaffold material is selected from one or more of the following: degradable protein or polypeptide materials, degradable polysaccharide materials, polyester hydrogels, polyacrylamide hydrogels such as poly (N-isopropylacrylamide) hydrogels, polyacrylic acid hydrogels and polyvinyl alcohol hydrogels.

[0017] Furthermore, the degradable protein or polypeptide material is selected from one or more of the following: collagen, fibronectin, laminin, elastin, silk fibroin, modified gelatin hydrogel such as methacrylated gelatin, modified silk fibroin hydrogel such as methacrylated silk fibroin and modified elastin hydrogel such as methacrylated elastin.

[0018] Furthermore, the degradable polysaccharide material is selected from one or more of the following: cellulose, chitin, hyaluronic acid, chondroitin sulfate, alginate, modified photosensitive chitin such as methacryloyl carboxymethyl chitosan, modified alginate hydrogel such as methacryloyl alginate, modified hyaluronic acid hydrogel such as methacryloyl hyaluronic acid, modified chondroitin sulfate hydrogel such as methacryloyl chondroitin sulfate and bacterial cellulose hydrogel.

[0019] Furthermore, the amino substitution degree of the methacryloyl gelatin is 30% to 90%, such as about 30%, about 60% or about 90%.

[0020] Furthermore, the concentration of the methacryloyl gelatin is 5% to 20%.

[0021] Furthermore, the concentration of the methacryloyl gelatin is 5% to 10%, such as about 5%, about 8% or about 10%.

[0022] According to another aspect of the present invention, a method for preparing the above-mentioned mesenchymal stem cell scaffold is provided, the method comprising the following steps:

[0023] (1) resuspending mesenchymal stem cells in a hydrogel to form a cell suspension; and

[0024] (2) forming the mesenchymal stem cell scaffold by 3D printing the cell suspension, or forming the mesenchymal stem cell scaffold by spreading the cell suspension in a culture dish / mold and cross-linking the cell suspension,

[0025] The number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed, or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increasing from the periphery of the scaffold to the center of the scaffold, or from one end of the scaffold to the other end of the scaffold.

[0026] Furthermore, in step (1), the cell density of the cell suspension is (0.01-10)×10 5 Pieces / ml.

[0027] Furthermore, the shape of the mesenchymal stem cell scaffold is suitable for the damaged area.

[0028] Furthermore, the shape is square, circular or oval.

[0029] Furthermore, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a mesenchymal stem cell scaffold with a bottom surface of about 5-20 mm×about 5-20 mm and a height of about 1-3 mm, or a mesenchymal stem cell scaffold with an upper bottom of about 3-15 mm×about 3-15 mm, a lower bottom of about 10-20 mm×about 10-20 mm, a height of about 1-3 mm, and a trapezoidal longitudinal section.

[0030] Furthermore, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a mesenchymal stem cell scaffold with a bottom surface of about 10 mm×about 10 mm and a height of about 1 mm, or a mesenchymal stem cell scaffold with an upper bottom of about 3 mm×about 3 mm, a lower bottom of about 10 mm×about 10 mm, a height of about 2 mm, and a trapezoidal longitudinal section.

[0031] Furthermore, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a filamentous material composed of one or more layers of silk threads.

[0032] Furthermore, the shape of the wire is a straight line or a curve.

[0033] Furthermore, the wire diameter of the wire is about 200 μm and / or the wire spacing is about 0.5-1.0 mm.

[0034] Furthermore, the threads are parallel and do not cross.

[0035] Furthermore, the wire material is a wire mesh material composed of triangles, quadrilaterals, pentagons, hexagons, circles or ellipses.

[0036] Furthermore, in step (2), the cross-linking conditions are: photo-cross-linking under a 405 nm light source for 10 to 30 seconds, and cross-linking 1 to 3 times.

[0037] Furthermore, in step (2), the cross-linking conditions are photo-cross-linking under a 405 nm light source for about 20 seconds, and cross-linking 3 times.

[0038] According to another aspect of the present invention, there is provided a method for preparing a new blood vessel network, the method comprising the following steps:

[0039] (1) transferring the aortic ring or aortic segment into the center of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method in the culture well;

[0040] (2) dropping 5 to 10% of a scaffold material onto the aortic ring or the aortic segment to embed the aortic ring or the aortic segment, and photocrosslinking for 10 to 30 seconds under a 405 nm light source;

[0041] (3) washing the culture well 1 to 3 times with vascular culture medium in a 37° C. incubator for 5 to 15 minutes each time; and

[0042] (4) co-culturing the vascular culture medium with the aortic ring or the aortic segment for 3 to 30 days to obtain the new

[0043] Vascular network.

[0044] Furthermore, before step (1), the above mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above method is pre-cultured in a mesenchymal stem cell culture medium containing 5-10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for 3-15 days.

[0045] Furthermore, before step (1), the above mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above method is pre-cultured in a mesenchymal stem cell culture medium containing about 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for 3 to 15 days.

[0046] Furthermore, before step (1), the above mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above method is precultured in a mesenchymal stem cell culture medium containing about 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for about 15 days.

[0047] Furthermore, in step (1), the aorta is flushed with vascular culture medium and then cut into aortic rings or aortic segments.

[0048] Furthermore, in step (1), the aortic ring or aortic segment is an aortic ring or aortic segment that has been starved overnight in a vascular culture medium.

[0049] Furthermore, the vascular culture medium is H-DMEM culture medium or vascular endothelial cell growth medium.

[0050] According to another aspect of the present invention, there is provided a use of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method or the neovascularization network prepared according to the above-mentioned method in preparing a product for preventing and / or treating ischemic and / or hypoxic diseases and / or injuries.

[0051] According to another aspect of the present invention, there is provided a use of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method or the neovascularization network prepared according to the above-mentioned method in preparing a product for preventing and / or treating fibrosis and / or scar formation.

[0052] According to another aspect of the present invention, there is provided a use of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method or the neovascularization network prepared according to the above-mentioned method in preparing a product for inducing angiogenesis.

[0053] Beneficial effects of the present invention:

[0054] The present invention uses mesenchymal stem cells and degradable biomaterials to prepare a scaffold for inducing angiogenesis, wherein the number of MSCs in the scaffold can be evenly distributed, or can gradually decrease from the center of the scaffold to the periphery, or from one end of the scaffold to the other end, in a gradient distribution, so that the concentration of its secretions (such as cytokines such as VEGF) also gradually decreases from the center of the scaffold to the periphery, or from one end of the scaffold to the other end, and this factor concentration gradient is used to better promote angiogenesis and extension. The scaffold can be applied to induce angiogenesis in ischemic and hypoxic parts of the heart and limbs, and has the prospect of improving microcirculation and blood and oxygen supply, and relieving and treating ischemic and hypoxic diseases. Compared with the previous method of inducing angiogenesis by simply using sustained-release microspheres encapsulating cytokines such as VEGF, PDGF, bFGF, etc., the MSCs scaffold can continuously secrete cytokines, which can not only induce angiogenesis, but also its potentials such as immunoregulation and fibrosis alleviation can further improve the microenvironment, promote angiogenesis and damage repair. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without exceeding the scope of protection required by the present invention.

[0056] Figure 1 Schematic diagram of the angiogenesis induced by the concentration gradient of MSCs and their paracrine factors in a mesenchymal stem cell (MSCs) scaffold. The rectangle represents the vascular ring, the circle represents MSCs, and the star represents the paracrine factor.

[0057] Figure 2 Schematic diagram of the MSCs scaffold prepared by 3D bioprinting in Example 1. A is the three-dimensional structure model of the MSCs non-gradient scaffold, BC is the 3D printed MSCs non-gradient scaffold; D is the three-dimensional structure model of the MSCs gradient scaffold, and EF is the 3D printed MSCs gradient scaffold.

[0058] Figure 3 Schematic diagram of the 3D printed MSCs scaffolds and vascular rings co-cultured with 2.5% FBS-added culture medium for 3, 7, and 12 days to induce angiogenesis and growth. MSCs are evenly distributed (A) or gradiently distributed (B) in the 3D printed scaffolds, and the scale bar = 500 μm.

[0059] Figure 4 This is an identification diagram of a vascular ring co-cultured with the MSCs gradient scaffold of Preparation Example 1 for 18 days. After fixation with paraformaldehyde, staining with BS1 lectin-FITC and DAPI was performed to mark vascular endothelial cells and cell nuclei, respectively. Scale bar = 500 μm. A shows new blood vessels (lectin-FITC marks vascular endothelial cells), B shows cell nuclei (DAPI marks), C shows vascular rings and new blood vessels (bright field), and D is a superimposed image of A and C.

[0060] Figure 5 The formation and growth of new blood vessels when the MSCs scaffolds pre-cultured for 10 days and the vascular rings were co-cultured in serum-free medium for 4 days, 12 days, and 30 days in Example 2. The MSCs scaffolds include GelMA60-MSCs uniform distribution scaffolds, GelMA60-MSCs gradient distribution scaffolds, and GelMA90-MSCs gradient distribution scaffolds, and the scale bar = 200 μm.

[0061] Figure 6The formation and growth of new blood vessels in the GelMA60-MSCs scaffold pre-cultured for 15 days in Example 3 were cultured with vascular rings for 4 days (A), 12 days (B), and 30 days (C, D) under serum-free conditions. Scale bar = 200 μm (AC), 500 μm (D). DETAILED DESCRIPTION

[0062] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0063] Unless otherwise specified, all technical and scientific terms and abbreviations used herein have the meanings commonly understood by those of ordinary skill in the field of the invention or the field in which the terms are used. Although preparation methods or materials similar to or equivalent to those disclosed herein may be used in the practice of the present invention, preferred preparation methods or materials are described herein.

[0064] As described in the background technology section, existing treatment methods have the problems of easily causing vascular reperfusion injury, multiple steps in the preparation of nanoparticle scaffold materials, complex processes, high prices, limited embedding efficiency, and high drug preparation costs. In order to solve the above problems, the present invention provides a mesenchymal stem cell scaffold for inducing angiogenesis, the mesenchymal stem cell scaffold comprises mesenchymal stem cells and scaffold materials, wherein the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increasing from the periphery of the scaffold to the center of the scaffold, or gradually increasing from one end of the scaffold to the other end of the scaffold.

[0065] To the extent that the terms "including, includes," "comprising, comprises," and "having, has, with" or variations thereof are used in the detailed description and / or claims, these terms are intended to be encompassed in a manner similar to the term "including, includes."

[0066] In the present invention, the prepared MSCs scaffold is cultured with complete medium for 1-2 weeks and used for in vitro research or in vivo transplantation. In in vitro research, the MSCs scaffold is co-cultured with endothelial cells or aortic vascular rings to detect the induction of angiogenesis. In vivo, the MSCs scaffold can be transplanted to the ischemic injury site, and the angiogenesis and injury repair of the injury site can be detected after 3-4 weeks.

[0067] In a preferred embodiment, the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold increases gradually from the periphery of the scaffold to the center of the scaffold, or increases gradually from one end of the scaffold to the other end of the scaffold.

[0068] In the present invention, given that MSCs have a strong paracrine capacity, the number gradient of MSCs will bring about a concentration gradient of its paracrine factors, thereby better inducing blood vessels to grow in the direction of high concentration. Under serum-free culture conditions, compared with uniformly distributed scaffolds, the length and daily average growth rate of new blood vessels in the vascular ring co-cultured with the gradient scaffold were significantly increased, indicating that the MSCs gradient scaffold can more effectively induce angiogenesis and growth than the MSCs uniformly distributed scaffold.

[0069] The implementation methods of the gradient scaffold of the present invention include the following two methods: (1) 3D printing, layer by layer, the style of the filling pattern inside each layer is not limited, it can be parallel filaments or polygonal grids, and the filament spacing, grid size, angle, etc. are adjusted according to different biological materials; a biological ink with a single cell density can be used for printing, or a plurality of biological inks with multiple cell densities can be used for multi-head controlled printing to achieve a gradient distribution of mesenchymal stem cells from the periphery to the center or from one end to the other end in the formed biological scaffold; (2) a biological ink with a single cell density is used, or a plurality of biological inks with multiple cell densities are prepared at the same time, added to a specific model or mold, and cross-linked by a suitable method to achieve a gradient distribution of mesenchymal stem cells from the periphery to the center or from one end to the other end in the formed biological scaffold.

[0070] In a preferred embodiment, the mesenchymal stem cells are selected from one or more of the following: bone marrow mesenchymal stem cells, peripheral blood mesenchymal stem cells, adipose mesenchymal stem cells, umbilical cord mesenchymal stem cells, umbilical cord blood mesenchymal stem cells, amniotic fluid mesenchymal stem cells, tooth mesenchymal stem cells, testicular mesenchymal stem cells, skin mesenchymal stem cells and placental mesenchymal stem cells.

[0071] In a preferred embodiment, the mesenchymal stem cells are autologous mesenchymal stem cells and / or allogeneic mesenchymal stem cells.

[0072] In a preferred embodiment, the autologous source is autologous peripheral blood and / or adipose tissue.

[0073] In a preferred embodiment, the allogeneic source is allogeneic umbilical cord Wharton's jelly, umbilical cord blood, amniotic fluid and / or placenta.

[0074] In a preferred embodiment, the mesenchymal stem cells secrete one or more substances selected from the group consisting of: soluble cytokines, microRNAs and exosomes.

[0075] In a preferred embodiment, the soluble cytokine is selected from one or more of the following: vascular endothelial growth factor, platelet-derived growth factor, basic fibroblast growth factor, hepatocyte growth factor, stromal cell-derived factor and insulin-like growth factor.

[0076] In a preferred embodiment, the scaffold material is a degradable biomaterial.

[0077] In a preferred embodiment, the scaffold material is a partially degraded, modified compound.

[0078] In a preferred embodiment, the compound is a temperature-sensitive compound or a photosensitivity compound.

[0079] In a preferred embodiment, the scaffold material is selected from one or more of the following: degradable protein or polypeptide materials, degradable polysaccharide materials, polyester hydrogels, polyacrylamide hydrogels, polyacrylic acid hydrogels and polyvinyl alcohol hydrogels.

[0080] In a preferred embodiment, the polyacrylamide hydrogel is poly(N-isopropylacrylamide) hydrogel.

[0081] In a preferred embodiment, the degradable protein or polypeptide material is selected from one or more of the following: collagen, fibronectin, laminin, elastin, silk fibroin, modified gelatin hydrogel, modified silk fibroin hydrogel and modified elastin hydrogel.

[0082] In a preferred embodiment, the modified gelatin hydrogel is methacrylated gelatin.

[0083] In a preferred embodiment, the modified silk fibroin hydrogel is methacrylylated silk fibroin.

[0084] In a preferred embodiment, the modified elastin hydrogel is methacrylylated elastin.

[0085] In a preferred embodiment, the degradable polysaccharide material is selected from one or more of the following: cellulose, chitin, hyaluronic acid, chondroitin sulfate, alginate, modified photosensitive chitin, modified alginate hydrogel, modified hyaluronic acid hydrogel, modified chondroitin sulfate hydrogel and bacterial cellulose hydrogel.

[0086] In a preferred embodiment, the modified photosensitive chitin is methacryloyl carboxymethyl chitosan.

[0087] In a preferred embodiment, the modified alginate hydrogel is methacrylated alginate.

[0088] In a preferred embodiment, the modified hyaluronic acid hydrogel is methacryloyl hyaluronic acid.

[0089] In a preferred embodiment, the modified chondroitin sulfate hydrogel is methacrylylated chondroitin sulfate.

[0090] In a preferred embodiment, the amino substitution degree of the methacryloyl gelatin is 30% to 90%.

[0091] In a preferred embodiment, the methacryloylated gelatin has an amino group substitution degree of about 30%.

[0092] In the present invention, "about" refers to a value within a range of ±5% of a specific value. For example, "about 30" includes ±5% of 30, or from 28.5 to 31.5, including 28.5 and 31.5.

[0093] In a preferred embodiment, the methacryloylated gelatin has an amino group substitution degree of about 60%.

[0094] In the present invention, "about" refers to a value within a range of ±5% of a specific value. For example, "about 60" includes ±5% of 60, or from 57 to 63, including 57 and 63.

[0095] In the present invention, compared with the GelMA90-MSCs gradient scaffold, the average length of new blood vessels induced by the GelMA60-MSCs gradient scaffold was significantly increased, indicating that the GelMA60-MSCs scaffold can more effectively induce angiogenesis and growth than the GelMA90-MSCs scaffold.

[0096] In a preferred embodiment, the methacryloylated gelatin has an amino group substitution degree of about 90%.

[0097] In the present invention, "about" refers to a value within the range of ±5% of a specific value. For example, "about 90" includes ±5% of 90, or from 85.5 to 94.5, including 85.5 and 94.5.

[0098] In a preferred embodiment, the concentration of the methacryloyl gelatin is 5% to 20%.

[0099] In the present invention, when the amino substitution degree, concentration, density, time, number of times, length, width, height, distance or other values ​​or parameters are expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when the range "5% to 20%" is disclosed, unless otherwise specified, the range is intended to include its end values ​​(e.g., 5% and 20%) and all integers (e.g., 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% and 19%) and non-integers within the range, and the technical effects of the present invention can be achieved within the above numerical range.

[0100] In a preferred embodiment, the concentration of the methacryloyl gelatin is 5% to 10%.

[0101] In a preferred embodiment, the concentration of the methacrylated gelatin is about 5%.

[0102] In the present invention, "about" refers to a value within the range of ±5% of a specific value. For example, "about 5" includes ±5% of 5, or from 4.75 to 5.25, including 4.75 and 5.25.

[0103] In a preferred embodiment, the concentration of the methacryloylated gelatin is about 8%.

[0104] In the present invention, "about" refers to a value within a range of ±5% of a specific value. For example, "about 8" includes ±5% of 8, or from 7.6 to 8.4, including 7.6 and 8.4.

[0105] In a preferred embodiment, the concentration of the methacrylated gelatin is about 10%.

[0106] In the present invention, "about" refers to a value within the range of ±5% of a specific value. For example, "about 10" includes ±5% of 10, or from 9.5 to 10.5, including 9.5 and 10.5.

[0107] According to another aspect of the present invention, a method for preparing the above-mentioned mesenchymal stem cell scaffold is provided, the method comprising the following steps:

[0108] (1) resuspending mesenchymal stem cells in a hydrogel to form a cell suspension; and

[0109] (2) forming the mesenchymal stem cell scaffold by 3D printing the cell suspension, or forming the mesenchymal stem cell scaffold by spreading the cell suspension in a culture dish / mold and cross-linking the cell suspension,

[0110] The number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed, or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increasing from the periphery of the scaffold to the center of the scaffold, or from one end of the scaffold to the other end of the scaffold.

[0111] In a preferred embodiment, in step (1), the cell density of the cell suspension is (0.01-10)×10 5 Pieces / ml.

[0112] In a preferred embodiment, the shape of the mesenchymal stem cell scaffold is square, circular, elliptical or a shape suitable for the damaged area.

[0113] In a preferred embodiment, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a mesenchymal stem cell scaffold with a bottom surface of about 5-20 mm×about 5-20 mm and a height of about 1-3 mm, or a mesenchymal stem cell scaffold with an upper bottom of about 3-15 mm×about 3-15 mm, a lower bottom of about 10-20 mm×about 10-20 mm, a height of about 1-3 mm, and a trapezoidal longitudinal section.

[0114] In a preferred embodiment, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a mesenchymal stem cell scaffold with a bottom surface of about 10 mm×about 10 mm and a height of about 1 mm, or a mesenchymal stem cell scaffold with an upper bottom of about 3 mm×about 3 mm, a lower bottom of about 10 mm×about 10 mm, a height of about 2 mm, and a trapezoidal longitudinal section.

[0115] In a preferred embodiment, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a filamentous material composed of one or more layers of silk threads.

[0116] In a preferred embodiment, the shape of the wire is a straight line or a curve.

[0117] In a preferred embodiment, the wire diameter of the wire is about 200 μm and / or the wire spacing is about 0.5-1.0 mm.

[0118] In a preferred embodiment, the threads are parallel and do not cross.

[0119] In a preferred embodiment, the wire material is a wire mesh composed of triangles, quadrilaterals, pentagons, hexagons, circles or ellipses.

[0120] In a preferred embodiment, in step (2), the cross-linking conditions are: photo-cross-linking under a 405 nm light source for 10 to 30 seconds, and cross-linking 1 to 3 times.

[0121] In a preferred embodiment, in step (2), the cross-linking condition is to cross-link for about 20 seconds under a 405 nm light source, and cross-link for 3 times.

[0122] According to another aspect of the present invention, there is provided a method for preparing a new blood vessel network, the method comprising the following steps:

[0123] (1) transferring an aortic ring or aortic segment starved overnight in serum-free H-DMEM medium into the center of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method in a culture well;

[0124] (2) dropping 5 to 10% of a scaffold material onto the aortic ring or the aortic segment to embed the aortic ring or the aortic segment, and photocrosslinking for 10 to 30 seconds under a 405 nm light source;

[0125] (3) washing the culture wells 1 to 3 times with H-DMEM medium in a 37° C. incubator for 5 to 15 minutes each time; and

[0126] (4) Adding H-DMEM culture medium containing 1-3 mM GlutaMAX and co-culturing with the aortic ring or the aortic segment for 3 to 30 days to obtain the new blood vessel network.

[0127] In a preferred embodiment, before step (1), the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method is pre-cultured in a mesenchymal stem cell culture medium containing 5-10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for 3-15 days.

[0128] In a preferred embodiment, before step (1), the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method is pre-cultured in a mesenchymal stem cell culture medium containing about 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for 3 to 15 days.

[0129] In a preferred embodiment, before step (1), the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method is precultured in a mesenchymal stem cell culture medium containing about 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for about 15 days.

[0130] In the present invention, the average length of blood vessels induced by the mesenchymal stem cell scaffold after about 15 days of pre-culture is significantly higher than the average length of blood vessels induced by the mesenchymal stem cell scaffold after 10 days of pre-culture. This may be because the growth state of MSCs in the scaffold is better after about 15 days of pre-culture, thereby being able to more effectively induce angiogenesis and growth.

[0131] In a preferred embodiment, in step (1), the aorta is flushed with vascular culture medium and then cut into aortic rings or aortic segments.

[0132] In a preferred embodiment, in step (1), the aortic ring or aortic segment is an aortic ring or aortic segment starved overnight in a vascular culture medium.

[0133] In the practical application of the present invention, starving the aortic ring overnight is not a necessary step. In the embodiment, the vascular ring is starved overnight in a serum-free medium and the MSCs scaffold is washed with a serum-free medium to remove the serum in these links, and then the MSCs scaffold is cultured in a serum-free manner to prove that the factors secreted by MSCs can induce the vascular ring to generate new blood vessels.

[0134] In a preferred embodiment, the vascular culture medium is H-DMEM culture medium or vascular endothelial cell growth medium.

[0135] In a preferred embodiment, in step (1), the amount of the 5-10% scaffold material added is 50-100 μl.

[0136] According to another aspect of the present invention, there is provided a use of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method or the neovascularization network prepared according to the above-mentioned method in preparing a product for preventing and / or treating ischemic and / or hypoxic diseases and / or injuries.

[0137] According to another aspect of the present invention, there is provided a use of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method or the neovascularization network prepared according to the above-mentioned method in preparing a product for preventing and / or treating fibrosis and / or scar formation.

[0138] According to another aspect of the present invention, there is provided a use of the above-mentioned mesenchymal stem cell scaffold or the mesenchymal stem cell scaffold prepared according to the above-mentioned method or the neovascularization network prepared according to the above-mentioned method in preparing a product for inducing angiogenesis.

[0139] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0140] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.

[0141] Example

[0142] 1. Isolation and culture of rat bone marrow derived MSCs (rBMSCs) rBMSCs were isolated from the femur and tibia bone marrow of SD rats and had strong adhesion to the wall. They were screened and isolated by the adherent culture method. After 3 days of primary culture, the cells showed a short spindle shape, growing individually and scatteredly on the wall; after 6 to 8 days of culture, the cells showed a typical long spindle shape of mesenchymal stem cells, and the cell density was high. The cell morphology of subcultured rBMSCs (P2 to P4) was uniform, with a typical long spindle shape and swirling growth.

[0143] In the following examples of the present invention, P4-P6 rBMSCs were used for experiments.

[0144] 2. Observation of MSCs culture and growth in GelMA

[0145] This experiment used methacrylic anhydride (MA) and gelatin to prepare photosensitive hydrogels - methacrylated gelatin (GelMA), with amino substitution degrees of 60% and 90%. L-DMEM containing 0.25% LAP was added and dissolved in a 50°C water bath to make a 5% hydrogel for the experiment.

[0146] rBMSCs from generation P4-P6 were resuspended in 5% GelMA60 or GelMA90 to make (1-10)×10 5 / ml cell suspension, added to 24-well plates, 0.3ml per well, cross-linked at 405nm for 60s. Add L-DMEM medium containing 10% FBS, incubate in a 37℃ incubator for 10min, wash twice, replace with fresh medium and culture every 3 days. Observation under an inverted microscope showed that MSCs began to spread after 3 days of culture in GelMA, and more cell morphology spread after 10 and 15 days of culture.

[0147] 3. Preparation of Rat Abdominal Aorta Vascular Rings

[0148] SD rats (100-150g, male) were anesthetized with ether and then killed by cervical dislocation. The chest and abdomen were disinfected with 70% ethanol, the chest cavity was opened, the internal organs were removed, the abdominal aorta was exposed, and the abdominal aorta was bluntly separated and transferred to pre-cooled H-DMEM containing 100 units / ml penicillin and 100μg / ml streptomycin. The fat and fibrous tissue on the outer layer of the blood vessels were carefully peeled off with microscissors and ophthalmic forceps, and the tiny blood vessel branches were cut off. The separated aorta was transferred to fresh pre-cooled H-DMEM, and the blood vessel cavity was flushed several times with a sterile syringe, cut into 1-2mm small segments, and transferred to new H-DMEM culture medium containing antibiotics and 2mM GlutaMAX, and cultured at 37°C overnight. During the whole process, it was noted that the aorta was immersed in the culture medium and kept moist.

[0149] 4. Preparation Example 1

[0150] 3D printed MSCs-loaded scaffolds and their in vitro angiogenesis-inducing effects

[0151] MSCs were resuspended in 8% GelMA to make 1×10 6 / ml cell suspension, made by 3D bioprinting technology: bottom surface 10×10mm 2 , MSCs are evenly distributed on the scaffold with a height of 0.927 mm (e.g. Figure 2 AC) and upper base 3×3mm 2 、Lower bottom 10×10mm 2 , 2 mm high, trapezoidal longitudinal section of MSCs gradient scaffold (such as Figure 2 DF), wire diameter 200μm, wire spacing 0.5mm. The printed scaffold was transferred to a 12-well culture plate, pre-cultured with L-DMEM medium containing 10% FBS for 4 days, replaced with serum-free HDMEM medium, washed twice in a 37°C incubator, incubated for 10min each time. The serum-free H-DMEM medium was aspirated, GelMA hydrogel was added around the scaffold, and photocrosslinked at 405nm for 20s to fix the scaffold in the center of the culture well. The rat abdominal aorta with peripheral connective tissue removed was cut into 1-2mm small segments, starved overnight in serum-free H-DMEM medium, transferred to each culture well, and the rat abdominal aorta ring was placed on one side of the scaffold with one end of the incision facing the scaffold. 5% GelMA was added to embed the vascular ring, and photocrosslinked at 405nm for 20s; washed twice in a 37°C incubator with fresh H-DMEM medium, 10min each time. Finally, H-DMEM medium containing 2.5% FBS and 2mM GlutaMAX was added and co-cultured with the aortic rings. The growth of new blood vessels on the vascular rings was observed under a microscope and photographed to analyze the complexity of vascular branching. The length of new blood vessels was measured using ImageJ software and the average daily growth rate was calculated.

[0152] The results are as follows Figure 3As shown in Tables 1 and 2, at 3, 7, and 12 days of culture, the length of the newly formed blood vessels in the vascular rings co-cultured with the MSCs gradient scaffolds was significantly greater than that in the vascular rings co-cultured with the MSCs uniformly distributed scaffolds (p<0.001). The average daily growth rates in the first 7 days were approximately 57.1% (3 days) and 131.3% (7 days) higher, respectively, indicating that the MSCs gradient scaffolds can better induce angiogenesis and growth.

[0153] Table 1 Average length (μm) and average daily growth rate (μm / day) of new blood vessels induced by 3D printed MSCs uniformly distributed scaffolds at different times

[0154]

[0155] Table 2 Average length (μm) and average daily growth rate (μm / day) of new blood vessels induced by 3D printed MSCs gradient distribution scaffolds at different times

[0156]

[0157] The vascular rings co-cultured with the MSCs gradient scaffold for 18 days were fixed with 4% paraformaldehyde at room temperature for 30 minutes, washed three times with PBS, each time for 15 minutes; incubated twice with 0.25% Triton X-100 at room temperature for 15 minutes each time, blocked with 5% BSA at room temperature for 1 hour, and washed three times with PBS, each time for 10 minutes. 10μg / ml BS1 lectin-FITC was added and incubated at 4℃ for 1-3 days, 1μg / ml DAPI was incubated at room temperature for 1 hour, and washed three times with PBS, each time for 10 minutes. Under a fluorescence microscope, new blood vessels were formed by green fluorescently labeled vascular endothelial cells and blue fluorescently labeled cell nuclei, extending from the periphery of the vascular rings (e.g. Figure 4 shown).

[0158] 5. Preparation Example 2

[0159] Study on the effect of MSCs-GelMA scaffold on inducing angiogenesis in rat aortic rings in vitro

[0160] MSCs were resuspended in 5% GelMA to make 2×10 5 / ml, 1×10 5 / ml, 5×10 4 / ml three concentrations of cell suspension, take 100μl respectively, and add the three concentrations of cell suspension in each culture well of the 24-well plate from the periphery to the center, so that the number of MSCs is the largest at the periphery and gradually decreases toward the center of the well, showing a gradient distribution. Take 100μl of the three concentrations of cell suspension respectively, mix by pipetting, and then add them to the culture well at one time, so that the number of MSCs tends to be evenly distributed in the culture well. Cross-link at 405nm for 3 times, each time for 20s, to make patches with MSCs in two states of gradient distribution and uniform distribution.

[0161] In this embodiment, GelMA used two different substitution degrees, namely GelMA60 and GelMA90. The prepared MSCs-GelMA60 patch and MSCs-GelMA90 patch were pre-cultured in L-DMEM culture medium supplemented with 10% FBS and 2mM GlutaMAX for 10 days, respectively, replaced with serum-free culture medium, washed twice in a 37°C incubator for 10 minutes each time, and then co-cultured with vascular rings in serum-free H-DMEM culture medium.

[0162] The rat aortic rings starved overnight in serum-free H-DMEM medium were transferred to each culture well and placed in the center of the MSCs patch. 5% GelMA was added to embed the vascular rings and cross-linked at 405nm for 20s. The H-DMEM was washed for 10min, and then H-DMEM medium containing 2mM GlutaMAX was added for culture. The medium was changed every 3 days. On the 4th day, new vascular branches were observed on the periphery of the arterial rings under a microscope. Photos were taken and the length of the new blood vessels was measured using ImageJ software to calculate the average daily growth rate.

[0163] The results are as follows Figure 5 As shown in Tables 3, 4 and 5, under serum-free culture conditions, the length and average daily growth rate of new blood vessels in the vascular rings co-cultured with the GelMA60-MSCs gradient scaffolds were higher than those in the MSCs uniform distribution group. After 12 days of co-culture, the length of the new blood vessels was significantly higher than that in the MSCs uniform distribution group (p<0.01), and the average daily growth rate was twice that of the MSCs uniform distribution group; after 30 days of co-culture, the length of the new blood vessels was also significantly higher than that in the MSCs uniform distribution group (p<0.05), and the average daily growth rate was about 28% higher than that of the MSCs uniform distribution group, indicating that the MSCs gradient scaffold can induce angiogenesis and growth more effectively than the MSCs uniform distribution scaffold.

[0164] Compared with the GelMA90-MSCs gradient scaffold, the average length of new blood vessels induced by the GelMA60-MSCs gradient scaffold was approximately 86.0% (4 days, p<0.001), 76.2% (12 days, p<0.05), and 54.0% (30 days, p<0.05) longer, and the average daily growth rate was approximately 86.2% (4 days), 70.2% (12 days), and 28.3% (30 days) higher, indicating that the GelMA60-MSCs scaffold can induce angiogenesis and growth more effectively than the GelMA90-MSCs scaffold.

[0165] Table 3 Average length (μm) and average daily growth rate (μm / day) of new blood vessels co-cultured with GelMA60-MSCs uniformly distributed scaffolds at different times

[0166]

[0167] Table 4 Average length (μm) and average daily growth rate (μm / day) of new blood vessels co-cultured with GelMA60-MSCs gradient scaffolds at different times

[0168]

[0169] Table 5 Average length (μm) and average daily growth rate (μm / day) of new blood vessels co-cultured with GelMA90-MSCs gradient scaffolds at different times

[0170]

[0171] 6. Preparation Example 3

[0172] Study on the effect of MSCs-GelMA scaffold on inducing angiogenesis in rat aortic rings in vitro

[0173] The MSCs-GelMA60 scaffolds were pre-cultured for 10 or 15 days and co-cultured with the vascular rings in serum-free medium for 4 days, 12 days, and 30 days. The formation and growth of new blood vessels: MSCs were resuspended in 5% GelMA60 to make 2×10 5 / ml, 1×10 5 / ml, 5×10 4 / ml three concentrations of cell suspension, take 100μl respectively, add the three concentrations of cell suspension from the periphery to the center in each culture well of the 24-well plate, cross-link at 405nm for 20s after each addition, cross-link 3 times in total, so that the number of MSCs is the largest at the periphery and gradually decreases toward the center of the well, showing a gradient distribution. Add 1ml of L-DMEM medium containing 10% FBS and 2mM GlutaMAX for culture, change the medium every 3-4 days, and pre-culture for 10 or 15 days. Change to serum-free medium and wash twice in a 37℃ incubator for 10min each time, and then co-culture with vascular rings in serum-free H-DMEM medium.

[0174] The rat aortic rings starved overnight in serum-free H-DMEM medium were transferred to each culture well and placed in the center of the MSCs scaffold that had been pre-cultured in vitro for 10 or 15 days. 5% GelMA was added to embed the cut segments and cross-linked at 405nm for 20s. The H-DMEM was washed for 10 minutes, and then H-DMEM medium containing 2mM GlutaMAX was added for culture. After 4, 12, and 30 days, the growth of new blood vessels on the arterial rings was observed under a microscope and photographed. The length of the new blood vessels was measured with ImageJ software, and the average daily growth rate was calculated.

[0175] The results are as follows Figure 6 As shown in Tables 6 and 7, the length and growth rate of the induced new blood vessels were significantly different after the GelMA60-MSCs scaffolds were pre-cultured for 10 or 15 days and then co-cultured with vascular rings in serum-free conditions. Among them, the average length of the blood vessels induced by the MSCs gradient scaffold pre-cultured for 15 days was approximately 115.4% (4 days, p<0.001), 41.3% (12 days, p<0.05), and 57.1% (30 days, p<0.05) higher than that of the 10-day pre-culture, respectively. This may be due to the better growth state of MSCs in the scaffold after 15 days of pre-culture, thereby more effectively inducing angiogenesis and growth.

[0176] Table 6 Average length (μm) and average daily growth rate (μm / day) of new blood vessels induced by MSCs scaffolds pre-cultured for 10 days

[0177]

[0178] Table 7 Average length (μm) and average daily growth rate (μm / day) of new blood vessels induced by MSCs scaffolds pre-cultured for 15 days

[0179]

[0180] The embodiments of the present invention are described in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, changes or deformations made by those skilled in the art based on the ideas of the present invention, the specific implementation methods and application scope of the present invention, all belong to the scope of protection of the present invention.

[0181] The present invention may be embodied in other specific forms without departing from the essential features of the present invention. The embodiments described are to be considered in all respects as illustrative rather than restrictive. The scope of the present invention is therefore indicated by the appended claims rather than by the foregoing description. In summary, the contents of this specification should not be construed as limiting the present invention.

Claims

1. A mesenchymal stem cell scaffold for inducing angiogenesis, characterized in that: The mesenchymal stem cell scaffold comprises mesenchymal stem cells and scaffold materials, wherein the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increased from the periphery of the scaffold to the center of the scaffold, or gradually increased from one end of the scaffold to the other end of the scaffold, so that the mesenchymal stem cells are gradually distributed in a gradient from the periphery to the center or from one end to the other end in the formed scaffold, thereby causing the concentration of secretions of the mesenchymal stem cells to gradually increase from the periphery to the center of the scaffold or from one end to the other end of the scaffold.

2. The mesenchymal stem cell scaffold according to claim 1, characterized in that: The mesenchymal stem cells are selected from one or more of the following: bone marrow mesenchymal stem cells, peripheral blood mesenchymal stem cells, adipose mesenchymal stem cells, umbilical cord mesenchymal stem cells, umbilical cord blood mesenchymal stem cells, amniotic fluid mesenchymal stem cells, tooth mesenchymal stem cells, testicular mesenchymal stem cells, skin mesenchymal stem cells and placental mesenchymal stem cells; Preferably, the mesenchymal stem cells are autologous mesenchymal stem cells and / or allogeneic mesenchymal stem cells; Preferably, the autologous source is autologous peripheral blood and / or fat; Preferably, the allogeneic source is allogeneic umbilical cord Wharton's jelly, umbilical cord blood, amniotic fluid and / or placenta; More preferably, the mesenchymal stem cells secrete one or more substances selected from the group consisting of: soluble cytokines, microRNAs, and exosomes; Also preferably, the soluble cytokine is selected from one or more of the following: vascular endothelial growth factor, platelet-derived growth factor, basic fibroblast growth factor, hepatocyte growth factor, stromal cell-derived factor and insulin-like growth factor.

3. The mesenchymal stem cell scaffold according to claim 1, characterized in that: The scaffold material is a degradable biomaterial; Preferably, the scaffold material is a partially degraded, modified compound such as a thermosensitive compound and / or a photosensitive compound; Preferably, the scaffold material is selected from one or more of the following: degradable protein or polypeptide materials, degradable polysaccharide materials, polyester hydrogels, polyacrylamide hydrogels such as poly (N-isopropylacrylamide) hydrogels, polyacrylic acid hydrogels and polyvinyl alcohol hydrogels; Preferably, the degradable protein or polypeptide material is selected from one or more of the following: collagen, fibronectin, laminin, elastin, silk fibroin, modified gelatin hydrogel such as methacrylated gelatin, modified silk fibroin hydrogel such as methacrylated silk fibroin and modified elastin hydrogel such as methacrylated elastin; Preferably, the degradable polysaccharide material is selected from one or more of the following: cellulose, chitin, hyaluronic acid, chondroitin sulfate, alginate, modified photosensitive chitin, such as methacryloyl carboxymethyl chitosan, modified alginate hydrogel such as methacryloyl alginate, modified hyaluronic acid hydrogel such as methacryloyl hyaluronic acid, modified chondroitin sulfate hydrogel such as methacryloyl chondroitin sulfate and bacterial cellulose hydrogel; More preferably, the amino substitution degree of the methacryloyl gelatin is 30% to 90%, such as about 30%, about 60% or about 90%; Particularly preferably, the concentration of the methacrylated gelatin is 5% to 20%; Particularly preferably, the concentration of the methacryloyl gelatin is 5% to 10%, such as about 5%, about 8% or about 10%.

4. A method for preparing the mesenchymal stem cell scaffold according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: (1) resuspending mesenchymal stem cells in a hydrogel to form a cell suspension; and (2) forming the mesenchymal stem cell scaffold by 3D printing the cell suspension, or forming the mesenchymal stem cell scaffold by spreading the cell suspension in a culture dish / mold and cross-linking the cell suspension, The number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is uniformly distributed, or the number of the mesenchymal stem cells in the mesenchymal stem cell scaffold is gradually increased from the periphery of the scaffold to the center of the scaffold, or gradually increased from one end of the scaffold to the other end of the scaffold, so that the mesenchymal stem cells are distributed in a gradient that gradually increases from the periphery to the center or from one end to the other end in the formed scaffold, thereby causing the concentration of secretions of the mesenchymal stem cells to gradually increase from the periphery to the center of the scaffold or from one end to the other end of the scaffold.

5. The method according to claim 4, characterized in that In step (1), the cell density of the cell suspension is (0.01-10)×10 5 Pieces / ml.

6. The method according to claim 4, characterized in that The shape of the mesenchymal stem cell scaffold is suitable for the damaged area; Preferably, the shape is square, circular or oval; Preferably, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a mesenchymal stem cell scaffold with a bottom surface of about 5 to 20 mm × about 5 to 20 mm and a height of about 1 to 3 mm, or a mesenchymal stem cell scaffold with an upper bottom of about 3 to 15 mm × about 3 to 15 mm, a lower bottom of about 10 to 20 mm × about 10 to 20 mm, a height of about 1 to 3 mm, and a trapezoidal longitudinal section; More preferably, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a mesenchymal stem cell scaffold with a bottom surface of about 10 mm×about 10 mm and a height of about 1 mm, or a mesenchymal stem cell scaffold with an upper bottom of about 3 mm×about 3 mm, a lower bottom of about 10 mm×about 10 mm, a height of about 2 mm, and a trapezoidal longitudinal section; Also preferably, in step (2), the mesenchymal stem cell scaffold formed by 3D printing is a filamentous material consisting of one or more layers of silk threads; Also preferably, the shape of the wire is a straight line or a curve; Preferably, the wire diameter of the wire is about 200 μm and / or the wire spacing is about 0.5-1.0 mm; Also preferably, the threads are parallel and do not cross; Also preferably, the wire material is a wire mesh material composed of triangles, quadrilaterals, pentagons, hexagons, circles or ellipses; Particularly preferably, in step (2), the cross-linking conditions are photo-cross-linking under a 405 nm light source for 10 to 30 seconds, and cross-linking 1 to 3 times; Particularly preferably, in step (2), the cross-linking conditions are photo-cross-linking under a 405 nm light source for about 20 seconds, and cross-linking 3 times.

7. A method for preparing a new blood vessel network, characterized in that: The method comprises the following steps: (1) transferring an aortic ring or an aortic segment into the center of the mesenchymal stem cell scaffold according to any one of claims 1 to 3 or the mesenchymal stem cell scaffold prepared by the method according to any one of claims 4 to 6 in a culture well; (2) dropping 5 to 10% of a scaffold material onto the aortic ring or the aortic segment to embed the aortic ring or the aortic segment, and photocrosslinking for 10 to 30 seconds under a 405 nm light source; (3) washing the culture wells 1 to 3 times with vascular culture medium in a 37° C. incubator for 5 to 15 minutes each time; and (4) co-culturing the vascular culture medium and the aortic ring or the aortic segment for 3 to 30 days to obtain the neovascular network; Preferably, before step (1), the mesenchymal stem cell scaffold according to any one of claims 1 to 3 or the mesenchymal stem cell scaffold prepared by the method according to any one of claims 4 to 6 is pre-cultured in a mesenchymal stem cell culture medium containing 5 to 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for 3 to 15 days; More preferably, before step (1), the mesenchymal stem cell scaffold according to any one of claims 1 to 3 or the mesenchymal stem cell scaffold prepared by the method according to any one of claims 4 to 6 is pre-cultured in a mesenchymal stem cell culture medium containing about 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for 3 to 15 days; More preferably, before step (1), the mesenchymal stem cell scaffold according to any one of claims 1 to 3 or the mesenchymal stem cell scaffold prepared by the method according to any one of claims 4 to 6 is pre-cultured in a mesenchymal stem cell culture medium containing about 10% serum or serum substitute, or in a mesenchymal stem cell serum-free culture medium for about 15 days; Preferably, in step (1), the aorta is flushed with vascular culture medium and then cut into aortic rings or aortic sections. part; Preferably, in step (1), the aortic ring or aortic segment is an aortic ring or aortic segment starved overnight in a vascular culture medium; Particularly preferably, the vascular culture medium is H-DMEM culture medium or vascular endothelial cell growth medium.

8. Use of the mesenchymal stem cell scaffold according to any one of claims 1 to 3, the mesenchymal stem cell scaffold prepared according to the method according to any one of claims 4 to 6, or the neovascularization network prepared according to the method according to claim 7 in preparing a product for preventing and / or treating ischemic and / or hypoxic diseases and / or injuries.

9. Use of the mesenchymal stem cell scaffold according to any one of claims 1 to 3, the mesenchymal stem cell scaffold prepared according to the method according to any one of claims 4 to 6, or the neovascularization network prepared according to the method according to claim 7 in preparing a product for preventing and / or treating fibrosis and / or scar formation.

10. Use of the mesenchymal stem cell scaffold according to any one of claims 1 to 3, the mesenchymal stem cell scaffold prepared by the method according to any one of claims 4 to 6, or the neovascularization network prepared by the method according to claim 7 in preparing a product for inducing angiogenesis.