High-absorptivity wet absorbent paper and preparation method thereof
Through the combination of the multi-layer structure of coniferous wood pulp and fluff pulp and PVA aqueous solution, the problems of limited water absorption and non-three-dimensional structure of water absorption paper are solved, and the effects of high liquid absorption and rapid diffusion are achieved, and the SAP polymer is maintained. Water absorption performance avoids falling off problems.
Patent Information
- Application Number
- CN202411157827.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing water-absorbing paper has limited water absorption, is not three-dimensional in structure, is slow in liquid diffusion, and polymer water-absorbing resin is prone to fall off during use.
Wet pulp is prepared by mixing coniferous wood pulp with fluff pulp, and through the multi-layer structure spreading and pressing composite technology, a structure is formed into a wet paper-SAP polymer-wet paper-SAP polymer-dry paper in sequence from top to bottom. The use of PVA aqueous solution is combined to improve water absorption performance and stereoscopicity.
The liquid absorption and looseness of the water-absorbing paper are improved, the structure is more three-dimensional, the liquid diffusion speed is accelerated, and the water absorption performance of the SAP polymer layer is maintained well, avoiding the problem of shedding.
Smart Images

Figure CN119041243A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sanitary products, and in particular to a highly absorbent wet-process absorbent paper and a preparation method thereof. Background Art
[0002] Polymer absorbent resin can absorb hundreds to thousands of times its own weight of water, has strong water absorption and water retention capacity, and is widely used in absorbent paper. At present, the common preparation methods of absorbent paper on the market include dry composite method and wet composite method. The dry composite method is to disperse the polymer absorbent resin on the surface of the wood pulp layer after spraying glue on the surface of the wood pulp layer. Since this absorbent paper is sprayed with glue, the water absorption capacity is low after drying, and the polymer absorbent resin is often found to fall off in disposable absorbent articles such as diapers or sanitary napkins, which poses certain hidden dangers. The existing wet absorbent paper is usually prepared by adding polymer absorbent resin at the initial stage of the wood pulp layer forming, and then covering it with a layer of dry paper for composite treatment. The absorbent paper obtained by this preparation method has low bulkiness, non-three-dimensional structure, slow liquid diffusion rate, and limited liquid absorption.
[0003] Chinese patent publication number CN109837801A discloses a high water absorption rate absorbent paper and a manufacturing method thereof, wherein the absorbent paper comprises a lower layer of paper, an upper layer of paper and absorbent resin (SAP) particles, wherein the lower layer of paper and the upper layer of paper are compounded in the wet part during papermaking on a papermaking machine, and absorbent resin (SAP) particles are uniformly added before compounding, and after the lower layer of paper and the upper layer of paper are compounded under pressure, the absorbent resin (SAP) particles are embedded in the compound area of the lower layer of paper and the upper layer of paper, and then the finished product is made by drying and rolling. The absorbent paper of the improved invention has the polymer absorbent resin (SAP) particles contained therein not exposed, but evenly embedded in the paper, and does not spill during use; the upper and lower surfaces of the absorbent paper of the invention are exposed to wood pulp, and the surface layer of wood pulp quickly absorbs water and diffuses it rapidly during the water absorption process, and the diffused water contacts and absorbs the polymer absorbent resin (SAP) particles, and the polymer absorbent resin (SAP) has a high water absorption rate and has a water-locking effect. However, the absorbent paper obtained by the invention has a structure of upper paper-middle absorbent resin particles-lower paper, which is relatively thin, has a limited water absorption capacity, is not three-dimensional, and has a slow liquid diffusion rate. Summary of the invention
[0004] Therefore, in view of the above problems, the present invention provides a highly absorbent wet-process absorbent paper and a preparation method thereof, which solves the defects of the absorbent paper obtained by the existing preparation method using the prior art, such as limited water absorption, non-three-dimensional structure and slow liquid diffusion speed.
[0005] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing highly absorbent wet-process absorbent paper, comprising the following preparation steps:
[0006] (1) Preparation of wet pulp: softwood pulp and fluff pulp are crushed and stirred respectively, and then the softwood pulp and fluff pulp are mixed in a weight ratio of 6-8:4-2 to obtain mixed pulp, and then a softener and a bulking agent are added to the mixed pulp, and the mixture is stirred and mixed to obtain wet pulp, and the wet pulp is pumped into a pulp storage tank;
[0007] (2) SAP spreading: The SAP polymer poured into the hopper is conveyed to the storage box of the polymer spreading device by a screw. The application amount is adjusted by controlling the rotation speed of the application roller and the depth of the surface groove. The application amount is controlled at 20-35g / m 2 , the temperature of the application roller is controlled at 48-52°C;
[0008] (3) Compounding: The wet pulp obtained in step (1) is conveyed through a felt cloth, initially squeezed to remove water, and then conveyed to the SAP polymer spreading section 1, where SAP polymer is spread online on the surface of the wet pulp, and a layer of dry paper is compounded online, and subjected to a pressure roller lamination process, wherein the pressure of the pressure roller is controlled at 0.3-0.5 MPa;
[0009] (4) Preliminary drying: The composite paper is transferred to a drying drum for preliminary drying. The drying temperature is controlled at 110-135°C to obtain a semi-dry semi-finished product having a surface layer of dry paper, a middle layer of SAP polymer, and a bottom layer of wet paper;
[0010] (5) using a wrinkling knife with an angle of 8-15° to peel the semi-dried semi-finished product off the drying drum so that it has a certain three-dimensional structure, and then transmitting it online after wrinkling;
[0011] (6) Secondary spreading of SAP: The wet pulp obtained in step (1) is conveyed to the second SAP polymer spreading section through another transmission line, and SAP is spread on the wet pulp, and the wet pulp is pressed by a pressure roller, wherein the pressure of the pressure roller is controlled at 0.3-0.5 MPa, and then subjected to a preliminary drying treatment to obtain wet paper with SAP polymer spread on the surface;
[0012] (7) the semi-finished product transmitted online in step (5) is turned over 180 degrees for transmission, so that the surface layer of the semi-finished product is wet paper, the middle layer is SAP polymer, and the bottom layer is dry paper, and the wet paper with SAP polymer sprinkled on the surface obtained in step (6) is then turned over 180 degrees for transmission and then composited with the semi-finished product to obtain a water-absorbing paper having a structure of wet paper-SAP polymer-wet paper-SAP polymer-dry paper from top to bottom;
[0013] (8) Drying: The absorbent paper is dried by a drying drum, the temperature of the drying drum is controlled at 110-135°C, and then peeled off the drying drum by a wrinkling knife at an angle of 8-15°, and transferred to an oven for drying. The moisture content is controlled at 5-10%, thereby obtaining a highly absorbent wet-process absorbent paper.
[0014] Furthermore, the method further comprises applying a PVA aqueous solution, wherein the PVA aqueous solution is prepared by dissolving PVA by stirring in water at 90-95°C, and the mass concentration of the PVA aqueous solution is 0.5-2%. The applying PVA aqueous solution is carried out during the compounding of step (3), and the specific process is as follows: the wet pulp obtained in step (1) is conveyed through a felt cloth, and a paper web is obtained after preliminary squeezing and dehydration, and the PVA aqueous solution is sprayed on the surface of the paper web, and the paper web is then conveyed to a SAP polymer spreading section 1, and SAP polymer is spread online on the surface of the paper web sprayed with the PVA aqueous solution, and a layer of dry paper is compounded online, and the paper web is subjected to a pressure roller pressing process, and the pressure of the pressure roller is controlled at 0.3-0.5Mpa.
[0015] Furthermore, the amount of the softener is 0.2-0.4% of the weight of the mixed pulp.
[0016] Furthermore: the dosage of the leavening agent is 0.1-0.3% of the weight of the mixed pulp.
[0017] Furthermore: the specific method of the drying treatment in step (8) is as follows: the hot air in the oven is the hot air heated by a heat exchanger, the hot air temperature is 120-150°C, the hot air enters from the top of the oven and blows downward, and the hot air passes through the paper surface and the conveyor belt to dry and remove water.
[0018] Furthermore, when the coniferous wood pulp and the fluff pulp are crushed separately, the pulping concentration is 3-7wt%, the pulping time is 15-30min, and no pulping process is used.
[0019] Further: the softener is polyoxyethylene stearate.
[0020] Further: the leavening agent is a mixture of sodium stearate and ethylenediamine in a weight ratio of 1:2-3.
[0021] A highly absorbent wet-laid absorbent paper, comprising a first wet-laid paper layer, a first SAP polymer layer, a second wet-laid paper layer, a second SAP polymer layer, and a dry paper layer stacked in sequence from top to bottom, wherein the first wet-laid paper layer and the second wet-laid paper layer have a bulkiness of 5-20 cm 3 / g.
[0022] Furthermore: a PVA layer is provided between the first wet-laid paper layer and the first SAP polymer layer.
[0023] By adopting the above technical solution, the beneficial effects of the present invention are:
[0024] 1. The highly absorbent wet-laid absorbent paper of the present invention uses coniferous wood pulp and fluff pulp as raw materials for the first and second wet-laid paper layers during the preparation process. Compared with the traditional paper using only wood pulp as raw material, it has higher bulkiness, faster diffusion speed and is softer.
[0025] 2. The absorbent paper obtained by the preparation method of highly absorbent wet-laid absorbent paper of the present invention comprises a first wet-laid paper layer, a first SAP polymer layer, a second wet-laid paper layer, a second SAP polymer layer, and a dry paper layer stacked in sequence from top to bottom. Compared with the traditional wet paper-SAP polymer layer-dry paper structure, the absorbent paper can absorb more liquid, has a higher liquid absorption amount, and has a more three-dimensional and bulky structure.
[0026] 3. In the preparation process of the present invention, a wrinkling knife with an angle of 8-15° is used to peel the semi-dry semi-finished product from the drying drum, so that it has a certain three-dimensional structure, and then it is transmitted online after wrinkling. The paper product obtained by this specific wrinkling treatment method has good three-dimensionality. Since the wrinkled structural layer-wet paper layer is an intermediate structural layer in the final structure of the absorbent paper, the absorbent paper finally obtained has a three-dimensional and fluffy structure, which is conducive to the rapid passage of liquid and accelerates the absorption speed of liquid.
[0027] 4. Furthermore, the absorbent paper of the present invention is sprayed with a layer of PVA aqueous solution before the SAP polymer is spread on the wet paper web. The PVA aqueous solution is rich in hydrophilic groups and can be dissolved in water. After the SAP is spread, it can, to a certain extent, play a role in blocking the direct contact between SAP and the wet paper web. During the initial drying (the initial drying temperature is 110-135°C), since the PVA has melted within this temperature range, it has a barrier effect on SAP, which can reduce the chance of water in the wet paper web generated in the subsequent processing process contacting with SAP, and play a certain protective role on SAP, so that the SAP in the finally obtained absorbent paper can maintain a relatively good water absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the structure of the highly absorbent wet-process absorbent paper in Example 1 of the present invention;
[0029] Figure 2 This is a schematic diagram of the preparation process of Example 1 of the present invention;
[0030] Figure 3 This is a schematic diagram of the preparation process of Example 2 of the present invention;
[0031] Figure 4 This is a schematic structural diagram of the highly absorbent wet-process absorbent paper in Example 2 of the present invention;
[0032] Figure 5 This is a schematic diagram of the preparation process of Example 3 of the present invention;
[0033] Figure 6 Schematic diagram of the structure of the highly absorbent wet-process absorbent paper in Example 3 of the present invention. DETAILED DESCRIPTION
[0034] Embodiment 1
[0035] refer to Figure 1 to Figure 2 , a method for preparing highly absorbent wet-process absorbent paper, comprising the following preparation steps:
[0036] (1) Preparation of wet pulp: softwood pulp and fluff pulp are crushed and stirred respectively, and then the softwood pulp and fluff pulp are mixed in a weight ratio of 6:4 to obtain mixed pulp, and then polyoxyethylene stearate, sodium stearate, and ethylenediamine are added to the mixed pulp, and the mixture is stirred and mixed to obtain wet pulp, which is then pumped into a pulp storage tank; the pulping concentration is 3wt%, and the pulping time is 15min; the amount of polyoxyethylene stearate is 0.2% of the weight of the mixed pulp, the amount of sodium stearate is 0.05% of the weight of the mixed pulp; and the amount of ethylenediamine is 0.1% of the weight of the mixed pulp;
[0037] (2) SAP spreading: The SAP polymer poured into the hopper is conveyed to the storage box of the polymer spreading device by a screw. The application amount is adjusted by controlling the rotation speed of the application roller and the depth of the surface groove. The application amount is controlled at 20g / m 2 , the temperature of the application roller is controlled at 48° C.;
[0038] (3) Compounding: The wet pulp obtained in step (1) is conveyed through a felt cloth, initially squeezed to remove water, and then conveyed to the SAP polymer spreading section 1, where SAP polymer is spread online on the surface of the wet pulp, and a layer of dry paper is compounded online, and subjected to a pressure roller lamination process, wherein the pressure of the pressure roller is controlled at 0.3 MPa;
[0039] (4) Preliminary drying: The composite paper is transferred to a drying drum for preliminary drying. The drying temperature is controlled at 110°C to obtain a semi-dry semi-finished product having a surface layer of dry paper, a middle layer of SAP polymer, and a bottom layer of wet paper;
[0040] (5) using a wrinkling knife with an angle of 8° to peel the semi-dried semi-finished product off the drying drum so that it has a certain three-dimensional structure, and then transmitting it online after wrinkling;
[0041] (6) Secondary spreading of SAP: The wet pulp obtained in step (1) is conveyed to the second SAP polymer spreading section through another transmission line, and SAP is spread on the wet pulp, and the wet pulp is pressed by a pressure roller, wherein the pressure of the pressure roller is controlled at 0.3 MPa, and then subjected to a preliminary drying treatment to obtain wet paper with SAP polymer spread on the surface;
[0042] (7) the semi-finished product transmitted online in step (5) is turned over 180 degrees for transmission, so that the surface layer of the semi-finished product is wet paper, the middle layer is SAP polymer, and the bottom layer is dry paper, and the wet paper with SAP polymer sprinkled on the surface obtained in step (6) is then turned over 180 degrees for transmission and then composited with the semi-finished product to obtain a water-absorbing paper having a structure of wet paper-SAP polymer-wet paper-SAP polymer-dry paper from top to bottom;
[0043] (8) Drying treatment: the absorbent paper is dried by a drying drum, the temperature of the drying drum is controlled at 110°C, and then peeled off the drying drum by an 8° wrinkling knife, and transferred to an oven for drying treatment, and the moisture content is controlled at 5%, thereby obtaining a highly absorbent wet-process absorbent paper. The specific method of the drying treatment is as follows: the hot air in the oven is the hot air heated by a heat exchanger, the temperature of the hot air is 120°C, the hot air enters from the upper part of the oven and blows downward, and the hot air passes through the paper surface and the conveyor belt to dry and remove water;
[0044] (9) Slitting and rolling.
[0045] A highly absorbent wet-laid absorbent paper obtained by the above preparation method has the following structure: a first wet-laid paper layer 1, a first SAP polymer layer 2, a second wet-laid paper layer 3, a second SAP polymer layer 4, and a dry paper layer 5 are stacked in sequence from top to bottom, and the first wet-laid paper layer 1 and the second wet-laid paper layer 3 both have high fluffiness, with a fluffiness of 7 cm 3 / g.
[0046] Embodiment 2
[0047] refer to Figure 3 and Figure 4 Compared with Example 1, the preparation method of a highly absorbent wet-process absorbent paper of this embodiment is different from that of Example 1 in step (3), and the other schemes are the same as those of Example 1. Specifically, the compounding process of step (3) is as follows: the wet pulp obtained in step (1) is conveyed through a felt cloth, and a paper web is obtained after preliminary squeezing and dehydration, the PVA aqueous solution is sprayed on the surface of the paper web, and the paper web is then transferred to SAP polymer spreading section 1, SAP polymer is spread online on the surface of the paper web sprayed with the PVA aqueous solution, a layer of dry paper is compounded online, and the paper web is subjected to pressure roller lamination treatment, the pressure of the pressure roller is controlled at 0.3-0.5Mpa, the PVA aqueous solution is prepared by dissolving PVA by stirring in 90°C water, and the mass concentration of the PVA aqueous solution is 1%.
[0048] The highly absorbent wet-process absorbent paper obtained by the above method has the following structure:
[0049] The first wet-laid paper layer 1, the PVA layer 6, the first SAP polymer layer 2, the second wet-laid paper layer 3, the second SAP polymer layer 4, and the dry paper layer 5 are stacked in sequence from top to bottom. The first wet-laid paper layer and the second wet-laid paper layer both have high fluffiness, with a fluffiness of 10 cm 3 / g.
[0050] Embodiment 3
[0051] refer to Figure 5 , Figure 6 And Example 2, a method for preparing a highly absorbent wet-process absorbent paper in this embodiment, before spreading SAP for the second time in step (6), a layer of PVA aqueous solution shown in Example 2 is sprayed on the wet paper web, and other technical solutions are the same as those in Example 2.
[0052] The absorbent paper obtained by the method has the following structure: a first wet-laid paper layer 1, a first PVA layer 6, a first SAP polymer layer 2, a second wet-laid paper layer 3, a second PVA layer 7, a second SAP polymer layer 4, and a dry paper layer 5 which are stacked in sequence from top to bottom.
[0053] Embodiment 4
[0054] A method for preparing highly absorbent wet-process absorbent paper comprises the following preparation steps:
[0055] (1) Preparation of wet pulp: softwood pulp and fluff pulp are crushed and stirred respectively, and then the softwood pulp and fluff pulp are mixed in a weight ratio of 8:2 to obtain mixed pulp, and then a softener and a bulking agent are added to the mixed pulp, and the mixture is stirred and mixed to obtain wet pulp, and the wet pulp is pumped into a pulp storage tank;
[0056] (2) SAP spreading: The SAP polymer poured into the hopper is conveyed to the storage box of the polymer spreading device by a screw. The application amount is adjusted by controlling the rotation speed of the application roller and the depth of the surface groove. The application amount is controlled at 35g / m 2 , the temperature of the application roller is controlled at 52° C.;
[0057] (3) Compounding: The wet pulp obtained in step (1) is conveyed through a felt cloth, initially squeezed to remove water, and then conveyed to the SAP polymer spreading section 1, where SAP polymer is spread online on the surface of the wet pulp, and a layer of dry paper is compounded online, and subjected to a pressure roller lamination process, wherein the pressure of the pressure roller is controlled at 0.5 MPa;
[0058] (4) Preliminary drying: The composite paper is transferred to a drying drum for preliminary drying. The drying temperature is controlled at 135°C to obtain a semi-dry semi-finished product having a surface layer of dry paper, a middle layer of SAP polymer, and a bottom layer of wet paper;
[0059] (5) using a wrinkling knife with an angle of 15° to peel the semi-dried semi-finished product off the drying drum so that it has a certain three-dimensional structure, and then transmitting it online after wrinkling;
[0060] (6) Secondary spreading of SAP: The wet pulp obtained in step (1) is conveyed to the second SAP polymer spreading section through another transmission line, and SAP is spread on the wet pulp, and the wet pulp is pressed by a pressure roller, wherein the pressure of the pressure roller is controlled at 0.5 MPa, and then subjected to a preliminary drying treatment to obtain wet paper with SAP polymer spread on the surface;
[0061] (7) Compounding the semi-finished product transferred online in step (5) onto the wet paper with SAP polymer sprinkled on the surface transferred online in step (6) to obtain absorbent paper having a structure of dry paper-SAP polymer-wet paper-SAP polymer-wet paper from top to bottom;
[0062] (8) Drying treatment: The absorbent paper is dried by a drying drum, the temperature of the drying drum is controlled at 135°C, and then peeled off the drying drum by a 15° wrinkling knife, and transferred to an oven for drying treatment. The moisture content is controlled at 10%, thereby obtaining a highly absorbent wet-process absorbent paper.
[0063] In addition, the process of Example 4 can also be improved, for example, coating of PVA aqueous solution is added during the preparation process of Example 4.
[0064] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A method for preparing highly absorbent wet-process absorbent paper, characterized in that: The method comprises the following preparation steps: (1) Preparation of wet pulp: softwood pulp and fluff pulp are crushed and stirred respectively, and then the softwood pulp and fluff pulp are mixed in a weight ratio of 6-8:4-2 to obtain mixed pulp, and then a softener and a bulking agent are added to the mixed pulp, and the mixture is stirred and mixed to obtain wet pulp, and the wet pulp is pumped into a pulp storage tank; (2) SAP spreading: The SAP polymer poured into the hopper is conveyed to the storage box of the polymer spreading device by a screw. The application amount is adjusted by controlling the rotation speed of the application roller and the depth of the surface groove. The application amount is controlled at 20-35g / m 2 , the temperature of the application roller is controlled at 48-52°C; (3) Compounding: The wet pulp obtained in step (1) is conveyed through a felt cloth, initially squeezed to remove water, and then conveyed to the SAP polymer spreading section 1, where SAP polymer is spread online on the surface of the wet pulp, and a layer of dry paper is compounded online, and subjected to a pressure roller lamination process, wherein the pressure of the pressure roller is controlled at 0.3-0.5 MPa; (4) Preliminary drying: The composite paper is transferred to a drying drum for preliminary drying. The drying temperature is controlled at 110-135°C to obtain a semi-dry semi-finished product having a surface layer of dry paper, a middle layer of SAP polymer, and a bottom layer of wet paper; (5) using a wrinkling knife with an angle of 8-15° to peel the semi-dried semi-finished product off the drying drum so that it has a certain three-dimensional structure, and then transmitting it online after wrinkling; (6) Secondary spreading of SAP: The wet pulp obtained in step (1) is conveyed to the second SAP polymer spreading section through another transmission line, and SAP is spread on the wet pulp, and the wet pulp is pressed by a pressure roller, wherein the pressure of the pressure roller is controlled at 0.3-0.5 MPa, and then subjected to a preliminary drying treatment to obtain wet paper with SAP polymer spread on the surface; (7) the semi-finished product transmitted online in step (5) is turned over 180 degrees for transmission, so that the surface layer of the semi-finished product is wet paper, the middle layer is SAP polymer, and the bottom layer is dry paper, and the wet paper with SAP polymer sprinkled on the surface obtained in step (6) is then turned over 180 degrees for transmission and then composited with the semi-finished product to obtain a water-absorbing paper having a structure of wet paper-SAP polymer-wet paper-SAP polymer-dry paper from top to bottom; (8) Drying: The absorbent paper is dried by a drying drum, the temperature of the drying drum is controlled at 110-135°C, and then peeled off the drying drum by a wrinkling knife at an angle of 8-15°, and transferred to an oven for drying. The moisture content is controlled at 5-10%, thereby obtaining a highly absorbent wet-process absorbent paper.
2. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: The process also includes applying a PVA aqueous solution, wherein the PVA aqueous solution is prepared by dissolving PVA by stirring in water at 90-95°C, and the mass concentration of the PVA aqueous solution is 0.5-2%. The process is carried out in the compounding step (3), and the specific process is as follows: the wet pulp obtained in the step (1) is conveyed through a felt cloth, and a paper web is obtained after preliminary squeezing and dehydration, and the PVA aqueous solution is sprayed on the surface of the paper web, and the paper web is then conveyed to the SAP polymer spreading process 1, and the SAP polymer is spread online on the surface of the paper web sprayed with the PVA aqueous solution, and a layer of dry paper is compounded online, and the paper web is pressed by a pressure roller, and the pressure of the pressure roller is controlled at 0.3-0.5Mpa.
3. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: The amount of the softener used is 0.2-0.4% of the weight of the mixed pulp.
4. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: The dosage of the bulking agent is 0.1-0.3% of the weight of the mixed pulp.
5. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: The specific method of the drying treatment in step (8) is as follows: the hot air in the oven is the hot air heated by the heat exchanger, the hot air temperature is 120-150°C, the hot air enters from the top of the oven and blows downward, and the hot air passes through the paper surface and the conveyor belt to dry and remove water.
6. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: When the coniferous wood pulp and the fluff pulp are crushed separately, the pulping concentration is 3-7wt% and the pulping time is 15-30min.
7. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: The softener is polyoxyethylene stearate.
8. The method for preparing a highly absorbent wet-process absorbent paper according to claim 1, characterized in that: The leavening agent is a mixture of sodium stearate and ethylenediamine in a weight ratio of 1:2-3.
9. A highly absorbent wet-process absorbent paper, characterized in that: The invention comprises a first wet-laid paper layer, a first SAP polymer layer, a second wet-laid paper layer, a second SAP polymer layer, and a dry paper layer which are sequentially stacked from top to bottom, wherein the bulkiness of the first wet-laid paper layer and the second wet-laid paper layer is 5-20 cm 3 / g.
10. A highly absorbent wet-process absorbent paper according to claim 9, characterized in that: A PVA layer is further provided between the first wet-laid paper layer and the first SAP polymer layer.
Citation Information
Patent Citations
Paper diaper
CN102462586A
Preparation method for composite processed absorbent paper by using cylinder mould machine
CN108867149A
High-absorbency absorbent paper and manufacture method thereof
CN109837801A
Preparation technology of high-water-absorption breathable tissue raw paper material for puerperae
CN110172856A
Papermaking and composite processing technology for composite liquid absorbing material and equipment thereof
CN111379188A