Semiconductor structure and manufacturing method thereof
During the P-column manufacturing process of the super-junction MOSFET device, a barrier layer is formed on the inner wall of the trench and the surface of the target layer and an epitaxial filling process is performed step by step, the problems of the hollowing of the top seal and epitaxial filling layer are solved, and the device is improved Reliability and product yield.
Patent Information
- Application Number
- CN202411238655.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
In the P-column manufacturing process, existing superjunction MOSFET devices have problems with trench top sealing and internal cavity of epitaxial filling layer, resulting in reduced device reliability.
A barrier layer is formed on the inner wall of the trench and the surface of the target layer, and multiple epitaxial filling processes are performed step by step from the bottom of the trench to the top. By removing some of the barrier layers, an epitaxial filling layer is formed on the exposed inner wall to avoid the accumulation of epitaxial filling material. Ensure filling quality and avoid holes.
It effectively avoids the problems of hollowing on the top sealing of the trench and the internal cavity of the epitaxial filling layer, and improves the reliability of the device and product yield.
Smart Images

Figure CN119049975A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a semiconductor structure and a method for manufacturing the same. Background Art
[0002] Super junction metal oxide semiconductor field effect transistor (MOSFET) is a new type of power semiconductor device. It introduces super junction structure (Super Junction) based on the conventional vertical double diffused metal oxide semiconductor (Vertical Diffused Metal Oxide Semiconductor, VDMOS). Super junction MOSFET devices not only have the excellent characteristics of VDMOS, such as high input impedance, fast switching speed, high operating frequency, good voltage controllability, good thermal stability and simple driving circuit, but also overcome the disadvantage of VDMOS that the on-resistance increases sharply with the breakdown voltage. Among them, the manufacturing process of the P column in the super junction MOSFET device has a great influence on the overall performance and cost of the device.
[0003] In the related art, the manufacture of P-pillars usually adopts a multi-layer epitaxial process and a deep trench epitaxial filling process. However, the multi-layer epitaxial process usually uses multiple photolithography, multiple ion implantation and multiple push processes to form the P-pillar, which has the problems of complex process and high cost; in addition, the deep trench epitaxial filling process usually uses one trench etching and one epitaxial growth to form the P-pillar. Due to the large depth-to-width ratio of the trench, it is easy to have the problem of sealing the top of the trench, resulting in irregular voids formed inside the trench, thereby reducing the reliability of the device. Summary of the invention
[0004] Based on this, an embodiment of the present application provides a semiconductor structure and a manufacturing method thereof, so as to effectively avoid the problem of trench top sealing and the problem of voids inside the epitaxial filling layer, thereby improving product yield and improving device reliability.
[0005] In order to achieve the above-mentioned purpose, on the one hand, some embodiments of the present application provide a method for manufacturing a semiconductor structure. The manufacturing method includes: forming a target layer, the target layer having a groove; forming a barrier layer on the inner wall of the groove and the surface of the target layer; performing multiple epitaxial filling processes step by step from the bottom to the top of the groove until the groove is filled with the epitaxial filling layer; wherein a single epitaxial filling process includes: removing part of the barrier layer to expose at least part of the inner wall of the groove; and forming an epitaxial filling layer on the exposed inner wall of the groove.
[0006] In some embodiments, the single epitaxial filling process further includes: during the process of forming the epitaxial filling layer on the exposed inner wall of the trench, introducing a target gas into the trench to remove the epitaxial filling material on the surface of the barrier layer.
[0007] In some embodiments, the target gas includes hydrogen chloride gas.
[0008] In some embodiments, the barrier layer conformally covers the inner wall of the trench; and the thickness of the barrier layer gradually increases from the bottom to the top of the trench.
[0009] In some embodiments, the barrier layer forming process includes a furnace thermal oxidation process.
[0010] In some embodiments, the barrier layer is removed using a hydrogen baking process.
[0011] In some embodiments, when a portion of the barrier layer is removed, at least one of the following features is included:
[0012] The hydrogen flow rate range of the hydrogen baking process includes: 10slm~100slm;
[0013] The baking temperature range of the hydrogen baking process includes: 900℃~1200℃;
[0014] The furnace chamber pressure range of hydrogen baking process includes: 100Torr~600Torr;
[0015] The baking time range of the hydrogen baking process includes: 40s~120s.
[0016] In some embodiments, the method for manufacturing a semiconductor structure further includes: after the trench is fully filled with the epitaxial filling layer, grinding the surfaces of the epitaxial filling layer and the target layer so that the epitaxial filling layer retained in the trench constitutes a first conductive type column of the super junction structure; wherein the target layer includes a second conductive type epitaxial layer.
[0017] On the other hand, the present disclosure also provides a semiconductor structure according to some embodiments; the semiconductor structure includes a target layer and an epitaxial filling layer. The target layer has a groove; the epitaxial filling layer fills the groove; the epitaxial filling layer is formed by the manufacturing method of the semiconductor structure as described in any of the aforementioned embodiments of the present disclosure.
[0018] In some embodiments, the epitaxial filling layer includes a first conductivity type column; the target layer includes a second conductivity type epitaxial layer; and the epitaxial filling layer and the target layer form a super junction structure.
[0019] The embodiments of the present application may or at least have the following advantages:
[0020] In the embodiment of the present application, a barrier layer is formed on the inner wall of the trench and the surface of the target layer, and multiple epitaxial filling processes are performed from the bottom to the top of the trench. In each epitaxial filling process, part of the barrier layer is removed and an epitaxial filling layer is deposited on the exposed inner wall of the trench that is not covered by the barrier layer. By performing the removal process and the epitaxial process alternately multiple times, an epitaxial filling layer that fills the trench is gradually formed from bottom to top in the trench. In this way, the epitaxial filling layer is obtained by forming a barrier layer and performing multiple epitaxial filling processes in steps, which prevents the epitaxial filling material from accumulating on the surface of the target layer and the top of the trench, thereby avoiding the top sealing problem of the trench during the epitaxial filling process; in addition, the filling quality of the epitaxial filling layer in the trench is improved, and the internal void problem of the epitaxial filling layer is avoided, thereby improving the reliability of the device.
[0021] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 A flowchart of a method for manufacturing a semiconductor structure provided in some embodiments;
[0024] Figure 2 A flow chart of a single epitaxial filling process provided in some embodiments;
[0025] Figure 3 A flowchart of another method for manufacturing a semiconductor structure provided in some embodiments;
[0026] Figure 4 A flowchart of another method for manufacturing a semiconductor structure provided in some embodiments;
[0027] Figure 5 A schematic diagram of the structure of a target layer provided in some embodiments;
[0028] Figure 6 A schematic diagram of a structure obtained after forming a barrier layer provided in some embodiments;
[0029] Figure 7 A schematic diagram of a flow chart of step S300 provided in some embodiments;
[0030] Figure 8 A schematic diagram of a structure obtained after forming an epitaxial filling layer provided in some embodiments;
[0031] Fig. 9 A schematic diagram of the structure of a semiconductor structure provided in some embodiments.
[0032] Description of reference numerals:
[0033] 1-target layer, 11-substrate, 12-epitaxial layer, G-groove, 2-barrier layer, a-groove bottom region, b-groove wall region, c-groove corner region, A1-first target region, A2-second target region, 3-epitaxial filling layer, P-first conductive type column. DETAILED DESCRIPTION
[0034] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0036] It should be understood that when an element or layer is referred to as being "on," "adjacent to," or "connected to" other elements or layers, it may be directly on, adjacent to, connected to, or coupled to other elements or layers, or there may be intervening elements or layers. It should be understood that, although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, doping types, and / or portions, these elements, components, regions, layers, doping types, and / or portions should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type, or portion from another element, component, region, layer, doping type, or portion. Therefore, without departing from the teachings of the present application, the first element, component, region, layer, doping type, or portion discussed below may be represented as a second element, component, region, layer, or portion.
[0037] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that when the terms "consisting of" and / or "comprising" are used in this specification, the presence of the features, integers, steps, operations, elements and / or parts can be determined, but the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups is not excluded. At the same time, when used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0038] Embodiments of the invention are described herein with reference to cross-sectional views that are schematic representations of idealized embodiments (and intermediate structures) of the present application, such that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances are anticipated. Embodiments of the present application should not be limited to the specific shapes of the regions shown herein, but include deviations in shapes due to, for example, manufacturing techniques. Therefore, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shapes of the regions of the device, and do not limit the scope of the present application.
[0039] The embodiments of the present application provide a semiconductor structure and a method for manufacturing the same, so as to effectively avoid the problem of trench top sealing and the problem of voids inside the epitaxial filling layer, thereby improving product yield and enhancing device reliability.
[0040] In some embodiments, some embodiments of the present application provide a method for manufacturing a semiconductor structure; see Figure 1 , the manufacturing method includes the following steps S100~S300.
[0041] S100, forming a target layer, wherein the target layer has a groove.
[0042] S200, forming a barrier layer on the inner wall of the trench and the surface of the target layer.
[0043] S300, performing multiple epitaxial filling processes step by step from the bottom to the top of the trench until the trench is fully filled with the epitaxial filling layer.
[0044] For some examples, see Figure 2 The single epitaxial filling process in step S300 includes the following steps S311~S312.
[0045] S311, removing part of the barrier layer to expose at least part of the inner wall of the trench.
[0046] S312, forming an epitaxial filling layer on the exposed inner wall of the trench.
[0047] It should be noted that, in the process of performing multiple epitaxial filling processes step by step from the bottom to the top of the trench in step S300 , step S311 and step S312 are performed alternately until the trench is fully filled with the epitaxial filling layer.
[0048] In the embodiment of the present application, a barrier layer is formed on the inner wall of the trench and the surface of the target layer, and multiple epitaxial filling processes are performed from the bottom to the top of the trench. In each epitaxial filling process, part of the barrier layer is removed and an epitaxial filling layer is deposited on the exposed inner wall of the trench that is not covered by the barrier layer. By performing the removal process and the epitaxial process alternately multiple times, an epitaxial filling layer that fills the trench is gradually formed from bottom to top in the trench. In this way, the epitaxial filling layer is obtained by forming a barrier layer and performing multiple epitaxial filling processes in steps, which prevents the epitaxial filling material from accumulating on the surface of the target layer and the top of the trench, thereby avoiding the top sealing problem of the trench during the epitaxial filling process; in addition, the filling quality of the epitaxial filling layer in the trench is improved, and the internal void problem of the epitaxial filling layer is avoided, thereby improving the reliability of the device.
[0049] In some examples, the groove includes a first target area and a second target area distributed from the bottom to the top thereof; step S300 further includes the following steps S321 to S324.
[0050] S321, removing part of the barrier layer to expose the inner wall of the trench in the first target area.
[0051] S322, forming an epitaxial filling layer on the exposed inner wall of the trench in the first target area.
[0052] S323, removing the barrier layer for a second time to expose the inner wall of the groove in the second target area.
[0053] S324, forming an epitaxial filling layer on the exposed inner wall of the trench in the second target area.
[0054] In an embodiment of the present application, two epitaxial filling processes are performed based on the first target area and the second target area respectively, so as to divide the formation of the epitaxial filling layer into two steps, thereby effectively avoiding the internal void problem of the epitaxial filling layer; in addition, the barrier layer in the corner area of the groove is thinned in multiple epitaxial filling processes, thereby effectively avoiding the top sealing problem of the trench during the epitaxial filling process; in this way, the filling quality of the epitaxial filling layer is effectively improved, thereby improving the reliability of the device.
[0055] In some embodiments, step S100 includes the following steps S101 to S104.
[0056] S101, providing an initial target layer.
[0057] S102, forming a mask layer on one side of the initial target layer; the mask layer includes a mask pattern for defining a groove.
[0058] S103, etching the initial target layer based on the mask layer to form a groove in the initial target layer.
[0059] S104, removing the mask layer to obtain a target layer.
[0060] In some embodiments, see Figure 3 , the single epitaxial filling process also includes the following step S330.
[0061] S330, during the process of forming the epitaxial filling layer on the exposed inner wall of the trench, introducing a target gas into the trench to remove the epitaxial filling material on the surface of the barrier layer.
[0062] In an embodiment of the present application, during the process of forming the epitaxial filling layer, the target gas is introduced simultaneously to promptly remove the epitaxial filling material deposited on the surface of the barrier layer to ensure that there is no residual epitaxial filling material on the surface of the barrier layer, thereby effectively preventing the accumulation of epitaxial filling material at the top of the trench and avoiding the top sealing problem of the trench, thereby improving the product yield and device reliability.
[0063] In some embodiments, see Figure 4 , the method for manufacturing the semiconductor structure further includes the following step S400.
[0064] S400, after the trench is fully filled with the epitaxial filling layer, grinding the surfaces of the epitaxial filling layer and the target layer, so that the epitaxial filling layer remaining in the trench constitutes a first conductive type column of the super junction structure; wherein the target layer includes a second conductive type epitaxial layer.
[0065] In the embodiment of the present application, the barrier layer removal process and the epitaxial filling process of the epitaxial filling layer are performed alternately multiple times to form a first conductive type column with high filling quality (i.e., there is no problem of voids in the epitaxial filling layer) in the high aspect ratio trench of the super junction structure, thereby ensuring the high input impedance characteristics of the super junction structure, improving the voltage resistance performance of the semiconductor structure, and thus improving the reliability of the device.
[0066] It should be understood that although Figure 1~Figure 4 The steps in the flowchart are shown in sequence as indicated by the arrows, but these steps are not necessarily executed in the order indicated by the arrows. Unless otherwise specified in this document, there is no strict order restriction for the execution of these steps, and these steps can be executed in other orders. Moreover, Figure 1~Figure 4At least part of the steps may include multiple steps or multiple stages. These steps or stages are not necessarily performed at the same time, but can be performed at different times. The execution order of these steps or stages is not necessarily sequential, but can be performed in turn or alternately with other steps or at least part of the steps or stages in other steps.
[0067] In order to more clearly illustrate the manufacturing method of the semiconductor structure in some of the above embodiments, the following embodiments are combined with Figure 5~Figure 9 Understand.
[0068] In some embodiments, the manufacturing method includes steps S100 to S300.
[0069] In step S100, refer to Figure 5 , a target layer 1 is formed, and the target layer 1 has a groove G.
[0070] In some embodiments, step S100 includes the following steps S101 to S104.
[0071] In step S101, an initial target layer is provided.
[0072] In step S102 , a mask layer is formed on one side of the initial target layer; the mask layer includes a mask pattern for defining the trench G.
[0073] By way of example, the mask layer includes, but is not limited to, a photoresist layer.
[0074] In some examples, a method for forming a mask pattern of a mask layer includes: forming a dielectric layer on a side of the mask layer away from an initial target layer; etching the dielectric layer to obtain a dielectric pattern layer; and etching the mask layer based on the dielectric pattern layer to form a mask pattern.
[0075] By way of example, the material of the dielectric layer may be silicon monoxide (SiO), silicon dioxide (SiO 2 ) or silicon nitride (Si 3 N 4 ) or the like.
[0076] By way of example, the etching process of the dielectric layer includes but is not limited to a photolithography process.
[0077] By way of example, the etching process of the mask layer includes but is not limited to a dry etching process.
[0078] In step S103, please continue to refer to Figure 5 , the initial target layer is etched based on the mask layer to form a groove G in the initial target layer.
[0079] By way of example, the etching process of the initial target layer includes, but is not limited to, a photolithography process.
[0080] In step S104, please continue to refer to Figure 5 , remove the mask layer to obtain the target layer 1.
[0081] Illustratively, the removal process of the mask layer includes, but is not limited to, a debonding process.
[0082] In some examples, the target layer 1 includes a substrate 11 and an epitaxial layer 12 .
[0083] For example, the depth of the groove G ranges from 20 μm to 90 μm. The depth of the groove G may be, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm or 90 μm.
[0084] Please refer to Figure 5 The depth of the groove G refers to the dimension of the groove G in the first direction (eg, the Y direction).
[0085] For example, the opening width of the groove G ranges from 1 μm to 8 μm; the opening width of the groove G may be, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm.
[0086] Please refer to Figure 5 The opening width of the groove G refers to the size of the opening of the groove in the second direction (eg, X direction).
[0087] For example, please continue to see Figure 5 The value range of the inclination angle of the groove wall of the groove G relative to the first direction (for example, the Y direction) (i.e., the groove angle) includes 90°~120°; the inclination angle of the groove wall of the groove G relative to the first direction (for example, the Y direction) can be, for example, 90°, 100°, 110° or 120°.
[0088] For example, the thickness of the epitaxial layer 12 ranges from 25 μm to 100 μm; the thickness of the epitaxial layer 12 may be, for example, 25 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.
[0089] Please refer to Figure 5 The thickness of the epitaxial layer 12 refers to the size of the epitaxial layer 12 in a first direction (eg, Y direction).
[0090] Based on the above example, please continue to refer to Figure 5 , the trench G extends deep into but does not penetrate the epitaxial layer 12 .
[0091] For example, the substrate 11 can be made of semiconductor material, insulating material, conductor material or any combination thereof. The substrate 11 can be a single-layer structure or a multi-layer structure. For example, the substrate 11 can be a silicon (Si) substrate, a silicon germanium (SiGe) substrate, a silicon germanium carbon (SiGeC) substrate, a silicon carbide (SiC) substrate, a gallium arsenide (GaAs) substrate, an indium arsenide (InAs) substrate, an indium phosphide (InP) substrate or other III / V semiconductor substrates or II / VI semiconductor substrates. Or, for example, the substrate 11 can be a layered substrate including Si / SiGe, Si / SiC, silicon on insulator (SOI) or silicon germanium on insulator. Therefore, the type of substrate 11 should not limit the scope of protection of the present application.
[0092] It should be noted that the groove G is perpendicular to the (100) crystal plane of the substrate 11 .
[0093] In step S200, refer to Figure 6 , a barrier layer 2 is formed on the inner wall of the groove G and the surface of the target layer 1 .
[0094] By way of example, the barrier layer 2 includes but is not limited to an oxide layer; the material of the barrier layer 2 may be, for example, silicon dioxide (SiO 2 ) or the like.
[0095] In some embodiments, see Figure 6 In Figure (b), the barrier layer 2 conformally covers the inner wall of the groove G; the film thickness of the barrier layer 2 gradually increases from the bottom of the groove G to its top.
[0096] In some embodiments, the process for forming the barrier layer 2 includes a furnace thermal oxidation process.
[0097] In some embodiments, please refer to Figure 6 In FIG. 5( b ), the groove G includes a groove bottom area a, a groove wall area b and a groove corner area c extending from the bottom to the top.
[0098] It should be explained that in the process of forming the barrier layer 2, the process gas molecules are more likely to gather and adsorb at the groove corner region c at the top of the groove G, so the film formation rate of the barrier layer 2 is fastest in the groove corner region c, followed by the groove wall region b of the groove G, and the slowest is the groove bottom region a at the bottom of the groove G; therefore, please refer to Figure 6 In Figure (b), the film formation rate of the barrier layer 2 gradually increases from the bottom to the top of the trench G, so the film thickness gradually increases.
[0099] For example, the average film thickness of the barrier layer 2 in the groove bottom area a ranges from 20 A to 60 A; the average film thickness of the barrier layer 2 in the groove bottom area a can be, for example, 20 A, 30 A, 40 A, 50 A or 60 A.
[0100] For example, the average film thickness of the barrier layer 2 in the groove wall region b ranges from 65 Å to 90 Å; the average film thickness of the barrier layer 2 in the groove wall region b may be, for example, 65 Å, 70 Å, 80 Å or 90 Å.
[0101] For example, the average film thickness of the barrier layer 2 in the notch corner region c ranges from 95 A to 120 A; the average film thickness of the barrier layer 2 in the notch corner region c can be, for example, 95 A, 100 A, 110 A or 120 A.
[0102] For example, the ratio of the average film thickness of the barrier layer 2 in the groove bottom region a, the average film thickness in the groove wall region b, and the average film thickness in the groove corner region c may be 2:4:5, for example.
[0103] In step S300, refer to Figure 7 , multiple epitaxial filling processes are performed step by step from the bottom to the top of the trench G until the trench G is fully filled with the epitaxial filling layer 3.
[0104] It should be noted that the conductivity type of the epitaxial filling layer 3 is the first conductivity type; and the conductivity type of the epitaxial layer 12 is the second conductivity type.
[0105] For example, the first conductivity type is P type; the second conductivity type is N type.
[0106] For example, the materials of the epitaxial filling layer 3 and the epitaxial layer 12 include but are not limited to silicon (Si); the material of the epitaxial filling layer 3 is, for example, P-type silicon (P-Si); the material of the epitaxial layer 12 is, for example, N-type silicon (N-Si).
[0107] In some embodiments, the single epitaxial filling process includes the following steps S311-S312.
[0108] In step S311, refer to Figure 7 In Figures (b) and (d), part of the barrier layer 2 is removed to expose at least part of the inner wall of the trench G.
[0109] For example, the barrier layer 2 is removed by using a hydrogen baking (H2 Bake) process.
[0110] In some embodiments, when a portion of the barrier layer 2 is removed, at least one of the following features is included:
[0111] (1) The hydrogen flow rate range of the hydrogen baking process includes: 10slm~100slm.
[0112] For example, the hydrogen flow rate of the hydrogen baking process may be 10 slm, 20 slm, 30 slm, 40 slm, 50 slm, 60 slm, 70 slm, 80 slm, 90 slm or 100 slm, etc.
[0113] (2) The baking temperature range of the hydrogen baking process includes: 900℃~1200℃.
[0114] For example, the baking temperature of the hydrogen baking process may be 900° C., 1000° C., 1100° C., or 1200° C., etc.
[0115] (3) The furnace chamber pressure range of the hydrogen baking process includes: 100Torr~600Torr.
[0116] For example, the furnace chamber pressure of the hydrogen baking process may be 100 Torr, 200 Torr, 300 Torr, 400 Torr, 500 Torr, or 600 Torr, etc.
[0117] (4) The baking time range of the hydrogen baking process includes: 40 s~120 s.
[0118] For example, the baking time of the hydrogen baking process may be 40 s, 50 s, 60 s, 70 s, 80 s, 90 s, 100 s, 110 s or 120 s, etc.
[0119] In step S312, refer to Figure 7 In Figures (c) and (e), an epitaxial filling layer 3 is formed on the exposed inner wall of the trench G.
[0120] It should be noted that, in the process of performing multiple epitaxial filling processes step by step from the bottom to the top of the trench G in step S300 , step S311 and step S312 are performed alternately until the trench G is fully filled with the epitaxial filling layer 3 .
[0121] In some examples, the trench G includes a first target area A1 and a second target area A2 distributed from the bottom to the top thereof.
[0122] By way of example, the first target area A1 includes the groove bottom area a and the lower part of the groove wall area b of the groove G; the second target area A2 includes the upper part of the groove wall area b and the groove corner area c.
[0123] According to the above example, the multiple epitaxial filling processes performed step by step from the bottom to the top of the trench G in step S300 can be performed based on the first target area A1 and the second target area A2.
[0124] According to the above example, step S300 may also include steps S321 to S324.
[0125] In step S321, refer to Figure 7 In FIG. 5( b ), part of the barrier layer 2 is removed to expose the inner wall of the groove G in the first target area A1 .
[0126] It should be noted that removing part of the barrier layer 2 in step S321 includes: removing the barrier layer 2 in the groove bottom area a and the lower part of the groove wall area b, and thinning the barrier layer 2 in the upper part of the groove wall area b and the groove corner area c; to expose the inner wall of the groove G in the first target area A1, and thin the barrier layer 2 in the second target area A2.
[0127] In step S322, refer to Figure 7 In FIG. 5( c ), an epitaxial filling layer 3 is formed on the exposed inner wall of the trench G in the first target area A1 .
[0128] In step S323, refer to Figure 7 In FIG. 5( d ), the barrier layer 2 is removed for a second time to expose the inner wall of the groove G in the second target area A2 .
[0129] It should be noted that the second removal of the barrier layer 2 in step S323 includes: removing the barrier layer 2 in the groove wall area b and the groove corner area c to expose the inner wall of the groove G in the second target area A2.
[0130] In step S324, refer to Figure 7 In FIG. 5( e ), an epitaxial filling layer 3 is formed on the exposed inner wall of the trench G in the second target area A2 .
[0131] It should be noted that, in the embodiments of the present application, although the number of target areas is two (i.e., the first target area A1 and the second target area A2), the number of target areas can also be multiple (for example, the groove wall area b can also be divided into multiple sub-areas as target areas), and the present application does not limit the number of target areas; it can be understood that when the number of target areas is multiple, the manufacturing method of the semiconductor structure provided by the present application is still to perform multiple epitaxial filling processes in steps from the bottom to the top of the trench G.
[0132] In some embodiments, the single epitaxial filling process further includes the following step S330 .
[0133] In step S330, refer to Figure 7In Figures (c) and (e), during the process of forming the epitaxial filling layer 3 on the exposed inner wall of the trench G, a target gas is introduced into the trench G to remove the epitaxial filling material on the surface of the barrier layer 2.
[0134] In some embodiments, the target gas includes hydrogen chloride (HCl) gas.
[0135] It should be noted that, in some embodiments, please refer to Figure 8 After the trench G is filled with the epitaxial filling layer 3 in step S300 , the surface of the epitaxial filling layer 3 is higher than the surface of the target layer 1 .
[0136] In some embodiments, the method for manufacturing a semiconductor structure further includes the following step S400 .
[0137] In step S400, refer to Fig. 9 After the trench G is fully filled with the epitaxial filling layer 3, the surfaces of the epitaxial filling layer 3 and the target layer 1 are ground so that the epitaxial filling layer 3 retained in the trench G constitutes a first conductive type column P of the super junction structure; wherein the target layer 1 includes a second conductive type epitaxial layer 12.
[0138] For example, the polishing process of the epitaxial filling layer 3 includes but is not limited to a chemical mechanical polishing (Chemical Mechanical Polishing, CMP for short) process.
[0139] By way of example, the first conductive type pillar P is, for example, a P pillar.
[0140] The present application also provides a semiconductor structure according to some embodiments, which can be prepared by the manufacturing method of the semiconductor structure in some of the above embodiments. The semiconductor structure also has the technical advantages of the manufacturing method of the above semiconductor structure. It should be noted that the parts that are the same or corresponding to the above embodiments can refer to the corresponding description of the above embodiments, and will not be described in detail below.
[0141] In some embodiments, see Fig. 9 , the semiconductor structure includes a target layer 1 and an epitaxial filling layer 3. The target layer 1 has a trench G; the epitaxial filling layer 3 fills the trench G; the epitaxial filling layer 3 is formed by the manufacturing method of the semiconductor structure as described in any of the aforementioned embodiments of the present disclosure.
[0142] For example, the depth of the groove G ranges from 20 μm to 90 μm. The depth of the groove G may be, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm or 90 μm.
[0143] Please refer to Fig. 9The depth of the groove G refers to the dimension of the groove G in the first direction (eg, the Y direction).
[0144] For example, the opening width of the groove G ranges from 1 μm to 8 μm; the opening width of the groove G may be, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm.
[0145] Please refer to Fig. 9 The opening width of the groove G refers to the size of the opening of the groove in the second direction (eg, X direction).
[0146] For example, please continue to see Fig. 9 The value range of the inclination angle of the groove wall of the groove G relative to the first direction (for example, the Y direction) (i.e., the groove angle) includes 90°~120°; the inclination angle of the groove wall of the groove G relative to the first direction (for example, the Y direction) can be, for example, 90°, 100°, 110° or 120°.
[0147] For example, the thickness of the epitaxial layer 12 ranges from 25 μm to 100 μm; the thickness of the epitaxial layer 12 may be, for example, 25 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.
[0148] Please refer to Fig. 9 The thickness of the epitaxial layer 12 refers to the size of the epitaxial layer 12 in a first direction (eg, Y direction).
[0149] In some examples, the target layer 1 includes a substrate 11 and an epitaxial layer 12 .
[0150] For example, please continue to see Fig. 9 , the trench G extends deep into but does not penetrate the epitaxial layer 12 .
[0151] It should be noted that the groove G is perpendicular to the (100) crystal plane of the substrate 11 .
[0152] For example, the substrate 11 can be made of semiconductor material, insulating material, conductor material or any combination thereof. The substrate 11 can be a single-layer structure or a multi-layer structure. For example, the substrate 11 can be a silicon (Si) substrate, a silicon germanium (SiGe) substrate, a silicon germanium carbon (SiGeC) substrate, a silicon carbide (SiC) substrate, a gallium arsenide (GaAs) substrate, an indium arsenide (InAs) substrate, an indium phosphide (InP) substrate or other III / V semiconductor substrates or II / VI semiconductor substrates. Or, for example, the substrate 11 can be a layered substrate including Si / SiGe, Si / SiC, silicon on insulator (SOI) or silicon germanium on insulator. Therefore, the type of substrate 11 should not limit the scope of protection of the present application.
[0153] In some embodiments, please refer to Fig. 9 , the epitaxial filling layer 3 includes a first conductivity type column P; the target layer 1 includes a second conductivity type epitaxial layer 12; the epitaxial filling layer 3 and the target layer 1 form a super junction structure.
[0154] In some examples, substrate 11 is a second conductivity type substrate.
[0155] For example, the first conductivity type is P type; the second conductivity type is N type.
[0156] For example, the materials of the first conductive type column P and the epitaxial layer 12 include but are not limited to silicon (Si); the material of the epitaxial filling layer 3 is, for example, P-type silicon (P-Si); and the material of the epitaxial layer 12 is, for example, N-type silicon (N-Si).
[0157] In addition, it is worth mentioning that the manufacturing method of the semiconductor structure provided in the embodiment of the present application can be preferably used for the preparation of the P column (that is, the first conductive type column P) in the super junction structure. It should be noted that the super junction structure is a structure in which multiple vertical PN junctions are arranged, and the epitaxial layer (such as the epitaxial layer 12) in the super junction structure is thick and has a deep groove (such as the groove G), and an inversion layer (such as the epitaxial filling layer 3) with a conductivity type opposite to that of the epitaxial layer is formed in the deep groove; the P column refers to the inversion layer (such as the first conductive type column P) filled in the deep groove of the super junction structure.
[0158] In the embodiment of the present application, an epitaxial filling layer 3 is formed by repeatedly performing a barrier layer removal process and an epitaxial filling process of the epitaxial filling layer alternately, so as to form a first conductive type column P with high filling quality (i.e., there is no problem of epitaxial filling layer voids) in a high aspect ratio trench G of a super junction structure, so as to ensure the high input impedance characteristics of the super junction structure, improve the voltage resistance performance of the semiconductor structure, and thus improve the reliability of the device.
[0159] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0160] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A method for manufacturing a semiconductor structure, characterized in that: include: forming a target layer, wherein the target layer has a groove; forming a barrier layer on the inner wall of the groove and the surface of the target layer; Perform multiple epitaxial filling processes step by step from the bottom to the top of the trench until the trench is filled with the epitaxial filling layer; wherein a single epitaxial filling process includes: removing a portion of the barrier layer to expose at least a portion of the inner wall of the groove; The epitaxial filling layer is formed on the exposed inner wall of the trench.
2. The method for manufacturing a semiconductor structure according to claim 1, characterized in that: The single epitaxial filling process further includes: During the process of forming the epitaxial filling layer on the exposed inner wall of the trench, a target gas is introduced into the trench to remove the epitaxial filling material on the surface of the barrier layer.
3. The method for manufacturing a semiconductor structure according to claim 2, characterized in that: The target gas includes hydrogen chloride gas.
4. The method for manufacturing a semiconductor structure according to claim 1, characterized in that: The barrier layer conformally covers the inner wall of the groove; The thickness of the barrier layer gradually increases from the bottom to the top of the trench.
5. The method for manufacturing a semiconductor structure according to claim 4, characterized in that: The barrier layer forming process includes a furnace tube thermal oxidation process.
6. The method for manufacturing a semiconductor structure according to claim 4, characterized in that: The barrier layer is removed by a hydrogen baking process.
7. The method for manufacturing a semiconductor structure according to claim 6, characterized in that: When removing part of the barrier layer, at least one of the following features is included: The hydrogen flow rate range of the hydrogen baking process includes: 10slm~100slm; The baking temperature range of the hydrogen baking process includes: 900°C to 1200°C; The furnace chamber pressure range of the hydrogen baking process includes: 100 Torr~600 Torr; The baking time range of the hydrogen baking process includes: 40s~120s.
8. The method for manufacturing a semiconductor structure according to any one of claims 1 to 7, characterized in that: Also includes: After the trench is fully filled with the epitaxial filling layer, grinding the surfaces of the epitaxial filling layer and the target layer so that the epitaxial filling layer remaining in the trench constitutes a first conductive type column of a super junction structure; Wherein, the target layer includes a second conductivity type epitaxial layer.
9. A semiconductor structure, characterized in that: include: a target layer having a groove; An epitaxial filling layer, filling the trench completely; The epitaxial filling layer is formed by the method for manufacturing a semiconductor structure according to any one of claims 1 to 8.
10. The semiconductor structure according to claim 9, characterized in that: The epitaxial filling layer includes a first conductive type column; the target layer includes a second conductive type epitaxial layer; the epitaxial filling layer and the target layer form a super junction structure.