Preparation method for interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode
By using a very small amount of solvated ionic liquid LiG3 on the interface of Li6PS5Cl/lithium metal negative electrode, the decomposition reaction problem when the sulfide electrolyte comes into contact with metal lithium is solved, the interface stability and battery circulation performance are significantly improved, and the The commercialization process of all-solid-state lithium metal batteries.
Patent Information
- Application Number
- CN202411160086.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
When the sulfide electrolyte comes into contact with lithium metal, it is easy to decompose, resulting in an increase in interface impedance, a decrease in battery cycle stability, and the formation of lithium dendrites at the grain boundaries leads to internal short circuits, hindering the high energy density and commercialization of all-solid lithium metal batteries. process of transformation.
The Li6PS5Cl/lithium metal negative electrode interface is modified by a very small amount of solvated ionic liquid LiG3, and the growth of lithium dendrites is suppressed by forming a solid electrolyte layer (SEI) in situ, reducing interface impedance, and improving interface stability.
The interface impedance of the lithium negative electrode/electrolyte is significantly reduced, the interface stability of the lithium negative electrode/sulfide electrolyte is improved, and the cycle stability and safety of the battery are enhanced.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sulfide all-solid-state batteries, and specifically relates to Li 6 PS 5 Preparation method for interface modification of Cl electrolyte and lithium metal anode. Background Art
[0002] In order to explore solid electrolytes with conductivity comparable to that of liquid electrolytes, many scientific researchers have made great efforts. Among many solid electrolytes, sulfide electrolytes have attracted much attention due to their ultra-high ionic conductivity. However, during the contact between sulfide electrolytes and metallic lithium, the electrolytes are easily reduced by metallic lithium and decompose, resulting in increased interfacial impedance and decreased battery cycle stability. In addition, electrons tend to gather at grain boundaries, and lithium dendrites are usually formed at the grain boundaries of sulfide electrolytes, which eventually leads to internal short circuits and failure of the battery. To this end, various strategies have been explored to solve the lithium anode / electrolyte interface problem.
[0003] For example, patent CN118231752A discloses a nitrogen-chlorine-based solid electrolyte and its preparation method and application. The molecular formula of the nitrogen-chlorine-based solid electrolyte is LixZrNyClz. The nitrogen-chlorine-based solid electrolyte is prepared according to the following steps S1 or S2: S1: (1) First, according to the stoichiometric ratio of the elements in the nitrogen-chlorine-based solid electrolyte, metal chlorides containing Li and Zr are mixed and ball-milled to obtain a chloride solid electrolyte; (2) Then, according to the stoichiometric ratio of nitrogen, the metal nitride of Li is added to the chloride solid electrolyte again and ball-milled to obtain; S2: According to the stoichiometric ratio of each element, the metal chloride of Li and / or Zr and the metal nitride of Li are mixed and ball-milled to obtain.
[0004] For example, patent CN117477013A also discloses a sulfide solid electrolyte and its preparation method and application. The preparation method comprises the following steps: dry-mixing the raw materials for preparing the sulfide solid electrolyte to obtain a mixed powder; and high-temperature roller milling the mixed powder under air atmosphere to obtain the sulfide solid electrolyte.
[0005] Although the performance of sulfide solid electrolytes has been improved, the lithium negative electrode and interface problems still hinder the large-scale production and commercialization of high-energy-density all-solid-state lithium metal batteries. Therefore, obtaining low-interface resistance and safe, dendrite-free solid lithium metal batteries and improving the battery's cycle stability have become current research focuses. Summary of the invention
[0006] A very small amount of solvated ionic liquid LiG3 (G3 is triethylene glycol dimethyl ether, Li is lithium bis(trifluoromethanesulfonyl imide)) is used to modify the Li6PSsC1 / metal lithium anode interface. The growth of lithium dendrites is suppressed by in-situ formation of a solid electrolyte layer (SEI) on the surface of the lithium anode. The conductivity of the solvated ionic liquid is as high as 1.0x10 -3 S / m, good interfacial wettability, and good interfacial compatibility with sulfide electrolytes. It significantly reduces the interfacial impedance of lithium negative electrode / electrolyte and improves the interfacial stability of lithium negative electrode / sulfide electrolyte.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] A kind of Li 6 PS 5 The preparation method of the interface modification between Cl electrolyte and lithium metal negative electrode is characterized by comprising the following steps:
[0009] (1)Li 6 PS 5 Preparation of Cl electrolyte: Preparation of LiCl electrolyte by solid phase sintering method 6 PS 5 Cl solid electrolyte. 2 S (Alfa, 99.9%), P 2 S 5 (Macklin, 99.9%), LiCl (Aladdin, 99.9%) as the initial raw materials, weigh the raw materials according to the appropriate amount, then pour them into the ball mill jar and seal them, place them in the ball mill for ball milling, and finally, seal the ball milled materials in a quartz tube. Sinter in a muffle furnace, and grind the sintered electrolytic powder for use. (2) Preparation of LiG3 ionic liquid: Use molecular sieve (4A, Sigma-Aldrich) to reduce the water content in anhydrous triethylene glycol dimethyl ether (G3, 99.9%, Sigma-Aldric), place LiTFSI (99.95%, Aladdin) in a vacuum drying oven and dry it, then dissolve an appropriate molar ratio of LiTFSI in anhydrous triethylene glycol dimethyl ether, add 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, CAS: 655249-87-9, and stir magnetically to obtain LiG3 solvated ionic liquid.
[0010] (3) Pour the LPSCl electrolyte powder into an insulating sleeve and press it into shape, and then place it in plasma for treatment to obtain a Li6PS5Cl electrolyte containing amino groups on the surface.
[0011] (4) Then the lithium sheets are attached to both sides of the LPSCl electrolyte layer to assemble a Li / LPSCl / Li symmetric cell. The same method is used to prepare a Li(LiG3) / Li symmetric cell containing a solvated ionic liquid, and an appropriate amount of solvated ionic liquid (LiG3) is coated between the Li sheet and the LPSC1 electrolyte layer containing amino groups on the surface to obtain a lithium metal negative electrode precursor.
[0012] (5) The lithium metal negative electrode precursor is placed in a plasma for treatment under the same treatment conditions as step 3 to obtain a lithium metal negative electrode.
[0013] In order to study the effect of the solvated ionic liquid interface modification layer on the battery cycle performance, NCM622 was used to assemble the NCM622 / LPSCILi / (LiG3) all-solid-state battery. First, the NCM622 cathode material and the LPSCI electrolyte were weighed in a mass ratio of 70:30, and then ground evenly in a mortar to obtain a composite cathode. Then, the LPSC electrolyte powder was placed in an insulating mold with a diameter of 10 mm and pressed together. The composite cathode powder was attached to one side of the electrolyte and pressed together at a pressure of 150 MPa. 25 uL of LiG3 was dropped on the other side of the LPSCI particles and a metal lithium sheet was attached. The battery without LiG3 on the lithium negative electrode side was used as a control sample. The specific capacity of the battery depends on the loading amount of the active material, of which the loading amount of NCM622 is 6 mg. The above operations were all carried out in a glove box filled with Ar atmosphere (oxygen partial pressure <0.1 ppm, water partial pressure <0.1 ppm).
[0014] As a preferred technical solution of the present invention, in step (1), the Li 2 S:P 2 S 5 The molar ratio of MgO:LiCl is 4-6:0.5-1.5:1-3.
[0015] As a preferred technical solution of the present invention, in step (1), the ball milling time is 0.5 to 1.5 hours.
[0016] As a preferred technical solution of the present invention, in step (1), the calcination temperature is 500-600°C.
[0017] As a preferred technical solution of the present invention, in step (1), the calcination time is 20 to 60 minutes.
[0018] As a preferred technical solution of the present invention, in step (2), the molar ratio of LiTFSI, anhydrous triethylene glycol dimethyl ether and 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt is 1:4-5:0.2-0.5. As a preferred technical solution of the present invention, in step (2), the magnetic stirring time is 12-24h.
[0019] As a preferred technical solution of the present invention, the preparation method of plasma treatment in steps (3) and (5) is:
[0020] F1. Preparation stage: evenly spread the sample to be processed on the sample table in the plasma reaction chamber; use a vacuum pump to evacuate the reaction chamber to a low pressure state, with the pressure range of 20 mTorr to 50 mTorr.
[0021] F2. Ammonia introduction and plasma generation: Ammonia is introduced at a certain flow rate of 10-20 standard cubic centimeters per minute through a precision gas flow meter; the RF power supply is turned on and the power range is adjusted to 100 to 200 watts to generate a stable ammonia plasma. The RF frequency is set at 13.56 MHz, the processing time is 10-30 minutes, and the product is taken out.
[0022] As a preferred technical solution of the present invention, in step (4), the molar amount of the ionic liquid LiG3 added is 1.1*10-7 to 2.7*10 -7 .
[0023] Beneficial effects of the present invention:
[0024] (1) In order to solve the interfacial reaction problem between lithium metal anode and sulfide electrolyte, a very small amount of solvated ionic liquid LiG3 is used to improve the interfacial stability of LPSC1 / lithium metal anode. The growth of lithium dendrites is inhibited by in-situ forming a SEI film containing LF on the surface of lithium metal anode. This is because the allyl groups in the LiG3 solvated ionic liquid react with the amine groups on the surface of Li6PS5Cl electrolyte to undergo amino-ene addition reaction.
[0025] The reaction forms a tight isolation layer, which can effectively prevent direct contact between metallic lithium and sulfide electrolyte, thereby reducing the occurrence of interfacial reactions. At the same time, this isolation layer can also serve as part of the SEI film, helping to inhibit the growth of lithium dendrites.
[0026] (2) LiG3 solvated ionic liquid has good interfacial wettability and good interfacial compatibility with sulfide electrolytes, which can significantly reduce the interfacial impedance of lithium anode / electrolyte. This is because the allyl groups in LiG3 solvated ionic liquids can interact with Li 6 PS 5 After the amino-ene addition reaction of the amine groups on the surface of the Cl electrolyte, a tight isolation layer is formed. This isolation layer not only has good interfacial compatibility but also has good conductivity, so it can significantly reduce the interfacial impedance of the lithium negative electrode / electrolyte. DETAILED DESCRIPTION
[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods and effects according to the present invention are described in detail below in conjunction with the embodiments.
[0028] Example 1
[0029] A kind of Li 6 PS 5 The preparation method of the interface modification between Cl electrolyte and lithium metal negative electrode comprises the following steps:
[0030] (1)Li 6 PS 5 Preparation of Cl electrolyte: Preparation of LiCl electrolyte by solid phase sintering method 6 PS 5 Cl solid electrolyte. 2 S (Alfa, 99.9%), P 2 S 5 (Macklin, 99.9%), LiCl (Aladdin, 99.9%) were used as the starting materials. First, 229.75 g Li 2 S,222.273g P 2 S 5 , 84.78g LiCl raw material, then poured into the ball mill jar, sealed, placed in the ball mill, the speed was set to 100rpm, the ball milling time was 1h. Finally, the ball milled material was sealed in a quartz tube. Sintered at 550℃ in a muffle furnace for 30min, and the sintered electrolytic powder was finely ground for use.
[0031] (2) Preparation of LiG3 ionic liquid: First, molecular sieves (4A, Sigma-Aldrich) were used to reduce the water content in anhydrous triethylene glycol dimethyl ether (G3, 99.9%, Sigma-Aldric), and LiTFSI (99.95%, Aladdin) was placed in a vacuum drying oven at 100°C and dried for 12 hours. Then, 287.08 g of LiTFSI and 141.05 g of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt were dissolved in 813 mL of anhydrous triethylene glycol dimethyl ether and magnetically stirred for 18 hours to obtain LiG3 solvated ionic liquid.
[0032] (3) First, the LPSCl electrolyte powder is poured into an insulating sleeve and pressed into shape, and then placed in a plasma for treatment to obtain a Li6PS5Cl electrolyte containing amino groups on the surface.
[0033] F1. Preparation stage: evenly spread the sample to be processed on the sample table in the plasma reaction chamber; use a vacuum pump to evacuate the reaction chamber to a low pressure state of 35 mTorr.
[0034] F2. Ammonia introduction and plasma generation: Ammonia is introduced at a certain flow rate of 15 cubic centimeters per minute through a precision gas flow meter; the RF power supply is turned on and the power is adjusted to 150 watts to generate a stable ammonia plasma. The RF frequency is set at 13.56 MHz. The processing time is 20 minutes, and the product is taken out.
[0035] (4) Then the lithium sheets were attached to both sides of the LPSCl electrolyte layer to assemble a Li / LPSCl / Li symmetric battery. The same method was used to prepare a Li(LiG3) / Li symmetric battery containing a solvated ionic liquid. 25 μL of the solvated ionic liquid (LiG3) was coated between the Li sheet and the LPSC1 electrolyte layer containing amino groups on the surface to obtain a lithium metal anode precursor.
[0036] (5) The lithium metal negative electrode precursor is placed in a plasma for treatment under the same treatment conditions as step 3 to obtain a lithium metal negative electrode.
[0037] In order to study the effect of the solvated ionic liquid interface modification layer on the battery cycle performance, NCM622 was used to assemble the NCM622 / LPSCILi (LiG3) all-solid-state battery. First, the NCM622 cathode material and the LPSCI electrolyte were weighed in a mass ratio of 70:30, and then ground evenly in a mortar to obtain a composite cathode. Then, the LPSC electrolyte powder was placed in an insulating mold with a diameter of 10 mm and pressed together. The composite cathode powder was attached to one side of the electrolyte and pressed together at a pressure of 150 MPa. 25 uL of LiG3 was dropped on the other side of the LPSCI particles and a metal lithium sheet was attached. The battery without LiG3 on the lithium negative electrode side was used as a control sample. The specific capacity of the battery depends on the loading amount of the active material, of which the loading amount of NCM622 is 6 mg. The above operations were all carried out in a glove box filled with Ar atmosphere (oxygen partial pressure <0.1 ppm, water partial pressure <0.1 ppm).
[0038] At a current density of 0.1C, the initial discharge capacity of the NCM622 / LPSCI / i(LiG3) battery is as high as 126.5 mAh g -1 After 60 cycles, the capacity retention rate is still 80.3%.
[0039] Example 2
[0040] A kind of Li 6 PS 5 The preparation method of the interface modification of Cl electrolyte and lithium metal negative electrode is different from that of Example 1 in that: (1) 183.8 g Li 2 S,111.137g P 2 S 5 , 42.39g LiCl raw material, ball milling time is 0.5h,
[0041] The calcination temperature is 500°C and the calcination time is 20 min.
[0042] (2) 287.08 g of LiTFSI and 80.6 g of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide were dissolved in 727 mL of anhydrous triethylene glycol dimethyl ether and magnetically stirred for 12 h.
[0043] (3) Pour the LPSCl electrolyte powder into an insulating sleeve and press it into shape, and then place it in plasma for treatment to obtain a Li6PS5Cl electrolyte containing amino groups on the surface.
[0044] F1. Preparation stage: evenly spread the sample to be processed on the sample table in the plasma reaction chamber; use a vacuum pump to evacuate the reaction chamber to a low pressure state of 20 mTorr.
[0045] F2. Ammonia introduction and plasma generation: Ammonia is introduced at a certain flow rate of 10 cubic centimeters per minute through a precision gas flow meter; the RF power supply is turned on and the power is adjusted to 100 watts to generate a stable ammonia plasma. The RF frequency is set at 13.56 MHz, the processing time is 10 minutes, and the product is taken out.
[0046] (4) Then the lithium sheets were attached to both sides of the LPSCl electrolyte layer to assemble a Li / LPSCl / Li symmetric battery. The same method was used to prepare a Li(LiG3) / Li symmetric battery containing a solvated ionic liquid. 20 μL of the solvated ionic liquid (LiG3) was coated between the Li sheet and the LPSC1 electrolyte layer containing amino groups on the surface to obtain a lithium metal anode precursor.
[0047] (5) The lithium metal negative electrode precursor is placed in a plasma for treatment under the same treatment conditions as step 3 to obtain a lithium metal negative electrode.
[0048] At a current density of 0.1C, the initial discharge capacity of the NCM622 / LPSCI / i(LiG3) battery is as high as 122 mAh g -1 After 60 cycles, the capacity retention rate is still 78%.
[0049] Example 3
[0050] A kind of Li 6 PS 5 The preparation method of the interface modification of Cl electrolyte and lithium metal negative electrode is different from that of Example 1 in that: 275.7 g Li 2 S,333.41g P 2 S 5 ,127.17g LiCl raw material,
[0051] (1) Weigh 183.8 g Li 2 S,111.137g P 2 S 5 , 42.39g LiCl raw material, ball milling time is 1.5h, calcination temperature is 600℃, and calcination time is 60min.
[0052] (2) 287.08 g of LiTFSI and 201.5 g of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide were dissolved in 908 mL of anhydrous triethylene glycol dimethyl ether and stirred magnetically for 24 h.
[0053] (3) Pour the LPSCl electrolyte powder into an insulating sleeve and press it into shape, and then place it in plasma for treatment to obtain a Li6PS5Cl electrolyte containing amino groups on the surface.
[0054] F1. Preparation stage: evenly spread the sample to be processed on the sample table in the plasma reaction chamber; use a vacuum pump to evacuate the reaction chamber to a low pressure state of 50 mTorr.
[0055] F2. Ammonia introduction and plasma generation: Ammonia is introduced at a certain flow rate of 20 cubic centimeters per minute through a precision gas flow meter; the RF power supply is turned on and the power is adjusted to 200 watts to generate a stable ammonia plasma. The RF frequency is set at 13.56 MHz. The processing time is 30 minutes, and the product is taken out.
[0056] (4) Then the lithium sheets were attached to both sides of the LPSCl electrolyte layer to assemble a Li / LPSCl / Li symmetric battery. The same method was used to prepare a Li(LiG3) / Li symmetric battery containing a solvated ionic liquid. 50 μL of the solvated ionic liquid (LiG3) was coated between the Li sheet and the LPSC1 electrolyte layer containing amino groups on the surface to obtain a lithium metal anode precursor.
[0057] (5) Placing the lithium metal negative electrode precursor in plasma for treatment under the same treatment conditions as step 3 to obtain a lithium metal negative electrode.
[0058] At a current density of 0.1C, the initial discharge capacity of the NCM622 / LPSCI / i(LiG3) battery is as high as 118 mAh g -1 After 60 cycles, the capacity retention rate is still 75.5%.
[0059] Comparative Example 1
[0060] A kind of Li 6 PS 5 The preparation method of the interface modification of Cl electrolyte and lithium metal negative electrode is different from that of Example 1 in that: 275.7 g Li 2S,333.41g P 2 S 5 ,127.17g LiCl raw material,
[0061] (1) Weigh 229.75 g Li 2 S,222.273g P 2 S 5 ,84.78g LiCl raw material, ball milling time is 1h, calcination temperature is 550℃, and calcination time is 30min.
[0062] (2) Dissolve 287.08 g of LiTFSI in 813 mL of anhydrous triethylene glycol dimethyl ether and stir the mixture under magnetic stirring for 18 h.
[0063] (3) The amount of ionic liquid LiG3 added was 25 μL.
[0064] At a current density of 0.1C, the initial discharge capacity of the NCM622 / LPSCI / i(LiG3) battery is as high as 118 mAh g -1 After 60 cycles, the capacity retention rate is still 75.5%.
[0065] Comparative Example 2
[0066] A kind of Li 6 PS 5 The preparation method of the interface modification of Cl electrolyte and lithium metal negative electrode is different from that of Example 1 in that: 275.7 g Li 2 S,333.41g P 2 S 5 ,127.17g LiCl raw material,
[0067] (1) Weigh 183.8 g Li 2 S,111.137g P 2 S 5 , 42.39g LiCl raw material, ball milling time is 1.5h, calcination temperature is 600℃, and calcination time is 60min.
[0068] (2) Dissolve 287.08 g of LiTFSI in 727 mL of anhydrous triethylene glycol dimethyl ether and stir the mixture under magnetic stirring for 12 h.
[0069] (3) First, the LPSCl electrolyte powder is poured into an insulating sleeve and pressed into shape, and then placed in a plasma for treatment to obtain Li 6 PS 5 Cl electrolyte.
[0070] F1. Preparation stage: evenly spread the sample to be processed on the sample table in the plasma reaction chamber; use a vacuum pump to evacuate the reaction chamber to a low pressure state of 35 mTorr.
[0071] F2. Ammonia introduction and plasma generation: Ammonia is introduced at a certain flow rate of 15 cubic centimeters per minute through a precision gas flow meter; the RF power supply is turned on and the power is adjusted to 150 watts to generate a stable ammonia plasma. The RF frequency is set at 13.56 MHz. The processing time is 20 minutes, and the product is taken out.
[0072] (4) Then the lithium sheets are attached to both sides of the LPSCl electrolyte layer to assemble a Li / LPSCl / Li symmetric battery. The same method is used to prepare a Li(LiG3) / Li symmetric battery containing a solvated ionic liquid, and the surface of the LPSC1 electrolyte layer containing amino groups is placed between them to obtain a lithium metal negative electrode precursor.
[0073] (5) Placing the lithium metal negative electrode precursor in plasma for treatment under the same treatment conditions as step 3 to obtain a lithium metal negative electrode.
[0074] At a current density of 0.1C, the initial discharge capacity of the NCM622 / LPSCI / i(LiG3) battery is as high as 118 mAh g -1 After 60 cycles, the capacity retention rate is still 75.5%.
Claims
1. A method for preparing a Li6PS5Cl electrolyte and a lithium metal negative electrode interface modification, characterized in that: The following steps are involved: (1) Preparation of Li6PS5Cl electrolyte: Li6PS5Cl solid electrolyte was prepared by solid phase sintering method. Li2S (Alfa, 99.9%), P2S5 (Macklin, 99.9%), LiCl (Aladdin, 99.9%) were used as initial raw materials. The raw materials were weighed according to appropriate amount, poured into a ball milling jar, sealed, placed in a ball mill, and finally, the ball milled material was sealed in a quartz tube. Sintered in a muffle furnace, the sintered electrolytic powder was finely ground for later use. (2) Preparation of LiG3 ionic liquid: Molecular sieves (4A, Sigma-Aldrich) were used to reduce the water content in anhydrous triethylene glycol dimethyl ether (G3, 99.9%, Sigma-Aldric), and LiTFSI (99.95%, Aladdin) was placed in a vacuum drying oven for drying. Then, an appropriate molar ratio of LiTFSI was dissolved in anhydrous triethylene glycol dimethyl ether, and 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt, CAS: 655249-87-9, was added and magnetic stirring was performed to obtain LiG3 solvated ionic liquid. (3) Pour the LPSCl electrolyte powder into an insulating sleeve and press it into shape, and then place it in plasma for treatment to obtain a Li6PS5Cl electrolyte containing amino groups on the surface. (4) Then the lithium sheets are attached to both sides of the LPSCl electrolyte layer to assemble a Li / LPSCl / Li symmetric cell. The same method is used to prepare a Li(LiG3) / Li symmetric cell containing a solvated ionic liquid, and an appropriate amount of solvated ionic liquid (LiG3) is coated between the Li sheet and the LPSC1 electrolyte layer containing amino groups on the surface to obtain a lithium metal negative electrode precursor. (5) The lithium metal negative electrode precursor is placed in a plasma for treatment under the same treatment conditions as step 3 to obtain a lithium metal negative electrode. In order to study the effect of the solvated ionic liquid interface modification layer on the battery cycle performance, NCM622 was used to assemble the NCM622 / LPSCILi / (LiG3) all-solid-state battery. First, the NCM622 cathode material and the LPSCI electrolyte were weighed in a mass ratio of 70:30, and then ground evenly in a mortar to obtain a composite cathode. Then, the LPSC electrolyte powder was placed in an insulating mold with a diameter of 10 mm and pressed together. The composite cathode powder was attached to one side of the electrolyte and pressed together at a pressure of 150 MPa. 25 uL of LiG3 was dropped on the other side of the LPSCI particles and a metal lithium sheet was attached. The battery without LiG3 on the lithium negative electrode side was used as a control sample. The specific capacity of the battery depends on the loading amount of the active material, of which the loading amount of NCM622 is 6 mg. The above operations were all carried out in a glove box filled with Ar atmosphere (oxygen partial pressure <0.1 ppm, water partial pressure <0.1 ppm).
2. The method for preparing the interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode according to claim 1, characterized in that: In step (1), the molar ratio of Li2S:P2S5:LiCl is 4-6:0.5-1.5:1-3.
3. The preparation method of Li6PS5Cl electrolyte and lithium metal negative electrode interface modification according to claim 1, characterized in that: In step (1), the ball milling time is 0.5 to 1.5 h.
4. The method for preparing the interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode according to claim 1, characterized in that: In step (1), the calcination temperature is 500-600°C.
5. The preparation method of Li6PS5Cl electrolyte and lithium metal negative electrode interface modification according to claim 1, characterized in that: In step (1), the calcination time is 20 to 60 minutes.
6. The method for preparing the interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode according to claim 1, characterized in that: In step (2), the molar ratio of LiTFSI, anhydrous triethylene glycol dimethyl ether and 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt is 1:4-5:0.2-0.
5.
7. The method for preparing the interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode according to claim 1, characterized in that: In step (2), the magnetic stirring time is 12-24h.
8. The method for preparing the interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode according to claim 1, characterized in that: The preparation method of plasma treatment in the steps (3) and (5) is: F1. Preparation stage: evenly spread the sample to be processed on the sample table in the plasma reaction chamber; use a vacuum pump to evacuate the reaction chamber to a low pressure state, with the pressure range of 20 mTorr to 50 mTorr. F2. Ammonia introduction and plasma generation: Ammonia is introduced at a certain flow rate of 10-20 standard cubic centimeters per minute through a precision gas flow meter; the RF power supply is turned on and the power range is adjusted to 100 to 200 watts to generate a stable ammonia plasma. The RF frequency is set at 13.56 MHz, the processing time is 10-30 minutes, and the product is taken out.
9. The method for preparing the interface modification of Li6PS5Cl electrolyte and lithium metal negative electrode according to claim 1, characterized in that: In step (4), the molar amount of the ionic liquid LiG3 added is 1.1*10-7 to 2.7*10 -7 .
Citation Information
Patent Citations
Solid-like electrolyte for lithium metal battery and preparation method thereof
CN110911735A
High-strength solid electrolyte membrane and preparation method and application thereof
CN113363561A
Interpenetrating network structure layer and in-situ preparation method and application thereof
CN114292484A
Controllable preparation method of self-repairing polymer electrolyte
CN116845351A
Polymer solid electrolyte lithium ion secondary cell
WO2001047055A1
Cited By
Silicon negative plate, preparation method thereof and all-solid-state battery
CN121790315A
In-situ grain boundary modified solid electrolyte and preparation method and application thereof
CN122370477A
Sulfide solid electrolyte, preparation method thereof and all-solid-state lithium metal battery
CN122455914A