Preparation method of high-reliability copper-clad ceramic circuit board
By introducing laser ablation equipment to optimize the preparation of brazing material step and replacing the existing etching process, the reliability problem caused by the difference in thermal expansion coefficient of raw materials during the preparation process of AMB copper-clad ceramic circuit board is solved, and high efficiency and environmental protection are achieved. The manufacture of ceramic circuit boards has stable high insulation characteristics and high reliability.
Patent Information
- Application Number
- CN202411182551.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
During the preparation process, the existing AMB copper-clad ceramic circuit boards have cracked and failed due to the poor thermal expansion coefficient of the raw materials. The existing etching process is lengthy, high cost and unenvironmental, and cannot meet the high reliability requirements.
Use laser ablation equipment to optimize the preparation of brazing step, replacing the existing etching process, and realize accurate preparation of brazing step structure through high-temperature melt diffusion, dry film compression, exposure, development, copper etching and film removal processes, reducing the preparation of brazing step structure Use of dry film materials and chemical potions.
The rapid preparation of high-reliability copper-clad ceramic circuit board is achieved, reducing cost and environmental impact, ensuring that solder has no residue, controllable step size, and stable high insulation characteristics and high reliability.
Smart Images

Figure CN119053043A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a circuit board, and in particular to a method for preparing a high-reliability copper-clad ceramic circuit board. Background Art
[0002] AMB copper-clad ceramic substrate materials are widely used in semiconductor module device packaging with high power and high heat dissipation requirements due to their high thermal conductivity and high insulation properties. The preparation process of AMB copper-clad ceramic circuit boards mainly involves three raw materials, namely ceramic substrates, copper, and brazing materials. Among them, ceramics are mostly silicon nitride, aluminum nitride, and aluminum oxide. The thickness of general ceramics is ≤2mm. Brazing materials are mostly silver-copper-titanium or copper-titanium alloy materials. The thickness of general brazing materials is ≤0.05mm. Copper is mostly oxygen-free copper with a purity of more than 99.9%, and the thickness of general copper strips is ≤2mm. The thermal expansion coefficients of these three raw materials are very different. Ceramic cracking and failure often occur during severe temperature shock tests, which cannot meet the high reliability requirements of products such as automobiles. For high-reliability AMB copper-clad ceramic circuit board products, the common solution in the industry is to use the existing etching process system to generate a brazing material step structure with stress release relief in stress concentration areas such as line spacing to improve product reliability.
[0003] In the prior art, patent document CN116193724A discloses a method for improving the reliability of copper-clad ceramic circuit boards by generating solder steps using an existing etching process. During the preparation process, this method requires repeating the existing etching process, which is lengthy and cumbersome. In addition, a chemical etching method is selected to remove copper to achieve solder step etching, which results in uncontrollable size and unstable reliability. In addition, the amount of dry film materials and copper etching solutions used increases, which increases the production cost and is not environmentally friendly. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a high-reliability copper-clad ceramic circuit board. By introducing laser ablation equipment, the existing solder step preparation method is optimized, the use of dry film materials and developer, copper etching solution, and film removal solution in the existing scheme is reduced, and the cost is lower and more environmentally friendly.
[0005] The object of the present invention is achieved by: a method for preparing a high-reliability copper-clad ceramic circuit board, comprising the following steps: S1) Preparation of copper-clad ceramic substrate: The ceramic substrate is clad with high-purity oxygen-free copper using a high-temperature melt diffusion process to form a substrate; S2) Dry film lamination of copper-clad ceramic substrate: A layer of photosensitive dry film is simultaneously covered on both sides of the copper-clad ceramic substrate by a laminator, and the image of the film is transferred to the board surface by exposure; S3) Exposure and development of the dry film on the front side of the copper-clad ceramic substrate: Use a customized strip film for exposure, and remove the part not covered by the photoresist through the development process to form the required circuit pattern; S4) Etching of copper circuits on copper-clad ceramic substrates: The copper surface exposed by dissolving the dry film is etched away with acidic copper chloride etching solution to remove the metal parts not protected by the photoresist, thereby forming a precise circuit pattern; S5) Dry film removal of copper-clad ceramic circuit board: placing the copper-clad ceramic substrate after copper etching into the prepared quantitative alkaline solution for film removal; S6) Laser ablation of solder on copper-clad ceramic circuit boards: By introducing laser ablation equipment, the laser ablation equipment performs laser ablation at a specific position according to the preset solder step size and preset parameters of the product, removes the solder, and completes the preparation of the solder step structure; S7) Surface treatment and cleaning of copper-clad ceramic circuit boards: Sandblast the substrate circuits to roughen and clean the surface and remove surface oxides and dirt.
[0006] Furthermore, the step S6) specifically includes: placing the copper-clad ceramic circuit board on a workbench, turning on the vacuum suction to fix the product, using the CCD camera of the laser ablation equipment to identify the mark point on the product to achieve alignment, and then the laser ablation equipment performs laser ablation at a specific position according to the preset solder step size and preset parameters of the product to remove the solder. During the entire laser ablation process, a vacuum air knife and a water cooling device are configured to ensure that the vaporized substances generated during the solder ablation process will not contaminate the surface of the copper-clad ceramic circuit board product. After the solder ablation is completed, the vacuum suction is turned off.
[0007] Furthermore, in the step S6), the laser pulse frequency range of the laser ablation is 50KHz-2000KHz; the scanning speed range of the laser is 10mm / s-2000mm / s.
[0008] Furthermore, the vacuum pressure range in step S6) is -0.08MPa-0Mpa.
[0009] Furthermore, the temperature of the water cooling device is set to 0-20°C.
[0010] The present invention adopts the above technical scheme, and compared with the prior art, the beneficial effects are as follows: 1) by introducing laser ablation equipment, the existing solder step preparation method is optimized, and the use of dry film materials and developer, copper etching solution, and film removal solution in the existing scheme is reduced, which is lower in cost and more environmentally friendly; 2) by introducing laser ablation equipment, the existing solder step preparation method is optimized, and the dry film pressing, exposure, development, copper etching, and film removal processes in the existing scheme are removed, the process is streamlined, and rapid preparation is achieved; 3) by introducing laser ablation equipment, the existing solder step preparation method is optimized, and the solder step etching size and appearance in the process of etching the solder with the existing chemical solution are compared. Laser ablation is simple and controllable, and is not affected by the matching of the solder etching solution and the solder composition, which is convenient for the size consistency and solder residue-free solder step preparation process; 4) the copper-clad ceramic circuit board product containing the solder step prepared by the present method has no solder residue, the size of the solder step is controllable, and it has stable high insulation properties and high reliability in actual measurement. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 Flowchart of the present invention.
[0012] Figure 2 A schematic diagram of the process of the preparation method of the present invention.
[0013] Among them, 01 oxygen-free copper, 02 brazing material, 03 ceramic substrate, 04 dry film. DETAILED DESCRIPTION
[0014] like Figure 1-2 A method for preparing a high-reliability copper-clad ceramic circuit board is shown, comprising the following steps: S1) Preparation of copper-clad ceramic substrate: The ceramic substrate is clad with high-purity oxygen-free copper using a high-temperature melt diffusion process to form a substrate; S2) Dry film lamination of copper-clad ceramic substrate: A layer of photosensitive dry film is simultaneously covered on both sides of the copper-clad ceramic substrate by a laminator, and the image of the film is transferred to the board surface by exposure; S3) Exposure and development of the dry film on the front side of the copper-clad ceramic substrate: Use a customized strip film for exposure, and remove the part not covered by the photoresist through the development process to form the required circuit pattern; S4) Etching of copper circuits on copper-clad ceramic substrates: The copper surface exposed by dissolving the dry film is etched away with acidic copper chloride etching solution to remove the metal parts not protected by the photoresist, thereby forming a precise circuit pattern; S5) Dry film removal of copper-clad ceramic circuit board: placing the copper-clad ceramic substrate after copper etching into the prepared quantitative alkaline solution for film removal; S6) Laser ablation of solder on copper-clad ceramic circuit boards: By introducing laser ablation equipment to replace the existing copper etching process, the preparation of the solder step structure is completed. During the laser ablation process to remove the solder, the copper-clad ceramic circuit board is placed on the workbench, and the vacuum suction is turned on to fix the product. The CCD camera of the laser ablation equipment is used to identify the mark points on the product to achieve alignment. Then the laser ablation equipment performs laser ablation at a specific position according to the preset solder step size and preset parameters of the product to remove the solder. During the entire laser ablation process, a vacuum air knife and water cooling equipment are configured to ensure that the vaporized substances generated during the solder ablation process will not contaminate the surface of the copper-clad ceramic circuit board product. After the solder ablation is completed, the vacuum suction is turned off; The power range of the laser for laser ablation is 10W~1000W; the laser pulse frequency range is 50KHz~2000KHz; the pulse width of the laser pulse is 10fs~10ms; the scanning speed range of the laser is 10mm / s-2000mm / s; the laser scanning interval is 0.01mm~0.2mm; the vacuum pressure range is -0.08MPa-0Mpa; the water cooling equipment temperature is set to 0-20℃.
[0015] S7) Surface treatment and cleaning of copper-clad ceramic circuit boards: Sandblast the substrate circuits to roughen and clean the surface and remove surface oxides and dirt.
[0016] The invention discloses a method for preparing a high-reliability copper-clad ceramic circuit board. By introducing laser ablation equipment, the existing method for preparing a solder step is optimized, the use of dry film materials and developer, copper etching solution, and film removal solution in the existing solution is reduced, and the cost is lower and more environmentally friendly. The copper-clad ceramic circuit board product containing a solder step prepared by the method has no solder residue, the size of the solder step is controllable, and it has stable high insulation properties and high reliability according to actual measurements.
[0017] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.
Claims
1. A method for preparing a high-reliability copper-clad ceramic circuit board, It is characterized in that The following steps are involved: S1) Preparation of copper-clad ceramic substrate: The ceramic substrate is clad with high-purity oxygen-free copper using a high-temperature melt diffusion process to form a substrate; S2) Dry film lamination of copper-clad ceramic substrate: A layer of photosensitive dry film is simultaneously covered on both sides of the copper-clad ceramic substrate by a laminator, and the image of the film is transferred to the board surface by exposure; S3) Exposure and development of the dry film on the front side of the copper-clad ceramic substrate: Use a customized strip film for exposure, and remove the part not covered by the photoresist through the development process to form the required circuit pattern; S4) Etching of copper circuits on copper-clad ceramic substrates: The copper surface exposed by dissolving the dry film is etched away with acidic copper chloride etching solution to remove the metal parts not protected by the photoresist, thereby forming a precise circuit pattern; S5) Dry film removal of copper-clad ceramic circuit board: placing the copper-clad ceramic substrate after copper etching into the prepared quantitative alkaline solution for film removal; S6) Laser ablation of solder on copper-clad ceramic circuit boards: By introducing laser ablation equipment, the laser ablation equipment performs laser ablation at a specific position according to the preset solder step size and preset parameters of the product, removes the solder, and completes the preparation of the solder step structure; S7) Surface treatment and cleaning of copper-clad ceramic circuit boards: Sandblast the substrate circuits to roughen and clean the surface and remove surface oxides and dirt.
2. A method for preparing a high-reliability copper-clad ceramic circuit board according to claim 1, It is characterized in that The step S6) specifically includes: placing the copper-clad ceramic circuit board on a workbench, turning on the vacuum suction to fix the product, using the CCD camera of the laser ablation equipment to identify the mark point on the product to achieve alignment, and then the laser ablation equipment performs laser ablation at a specific position according to the preset solder step size and preset parameters of the product to remove the solder. During the entire laser ablation process, a vacuum air knife and a water cooling device are configured to ensure that the vaporized substances generated during the solder ablation process will not contaminate the surface of the copper-clad ceramic circuit board product. After the solder ablation is completed, the vacuum suction is turned off.
3. A method for preparing a high-reliability copper-clad ceramic circuit board according to claim 1, It is characterized in that The laser pulse frequency range of the laser ablation in step S6) is 50KHz-2000KHz; the scanning speed range of the laser is 10mm / s-2000mm / s.
4. A method for preparing a high-reliability copper-clad ceramic circuit board according to claim 1, It is characterized in that The pressure range of the vacuum suction in step S6) is -0.08MPa-0Mpa.
5. A method for preparing a high-reliability copper-clad ceramic circuit board according to claim 2, It is characterized in that The water cooling device temperature is set at 0-20°C.
Citation Information
Patent Citations
Method for laser-assisted manufacturing of precise circuit
CN114158195A
AMB copper-clad ceramic circuit board and preparation method thereof
CN116156772A
Method capable of integrally removing photosensitive dry film and copper-clad ceramic substrate solder layer
CN116647996A
Ceramic copper-clad plate as well as preparation method and application thereof
CN117769152A
Method for manufacturing metal-ceramic joined substrate
JP2013209237A
Cited By
AMB product with high recognition degree of PR target spot and preparation method of AMB product
CN119786353A
Manufacturing method of ceramic copper-clad carrier plate for lead-free soldering paste, ceramic copper-clad carrier plate and electronic equipment
CN120050853A