Preparation method and application of Na and K co-doped g-C3N5 photocatalyst
Through Na and K co-doping and crystallinity regulation methods, the electronic structure and energy band structure of g-C3N5 are optimized to form a small layer of ultra-thin nanosheet photo-autogenic Fenton catalyst, which solves the problem of insufficient photocatalytic activity of pure g-C3N5 , significantly improves H2O2 yield and photocatalytic properties.
Patent Information
- Application Number
- CN202411183372.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Pure nitride graphite carbon (g-C3N5) has weak photocatalytic activity in the production of hydrogen peroxide (H2O2), slow electron-hole pair dissociation, slow charge transfer mechanics, low oxygen reduction ability and scarce active sites. Its efficiency in photocatalytic production of H2O2 is limited.
Through Na and K co-doping and crystallinity regulation methods, the electronic structure and energy band structure of g-C3N5 are optimized, and a small layer of ultra-thin nanosheet light-automatic Fenton catalyst is formed, which increases carrier separation efficiency and introduces high oxygen content. Functional groups and polar hydroxyl groups increase n→π* electron transition and charge mobility, and activate more active sites.
The photocatalytic activity of g-C3N5 was significantly improved, and the H2O2 yield reached 122.15μmol g-1h-1, which was 11 times that of pure g-C3N5. It efficiently degrades antibiotics in a short time, improving the performance of photocatalysts and visible light absorption. ability.
Smart Images

Figure CN119056479A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a Na and K co-doped g-C3N5 photocatalyst, belonging to the technical field of composite photocatalytic materials. Background Art
[0002] With the rapid growth of global energy consumption and the intensification of environmental damage, environmental pollution is becoming more and more serious, and green energy is becoming more and more popular. Hydrogen peroxide (H2O2) has been widely used as a green energy in many fields such as chemical industry, wastewater purification and fuel cells due to the environmentally friendly, renewable and non-toxic properties of its decomposition products. Traditional H2O2 synthesis methods mainly rely on the anthraquinone process, which is plagued by problems such as waste accumulation, increased energy consumption and strict reaction requirements, which limit its sustainable production and production. Compared with the anthraquinone method, the photocatalytic two-electron oxygen reduction reaction is a more environmentally friendly and efficient synthetic route to generate H2O2. Under ambient conditions, water and oxygen undergo a photocatalytic reaction on the surface of a semiconductor to generate H2O2.
[0003] In this field, graphene nitride (g-C3N5) has attracted extensive attention due to its abundant electron-rich sites and basic nitrogen, especially the introduction of supplementary nitrogen in the triazine unit of g-C3N5, which expands its conjugated structure, higher thermodynamic stability, better electronic properties and narrower energy band. However, pure g-C3N5 still faces various shortcomings such as slow electron-hole pair dissociation, sluggish charge transfer kinetics, low oxygen reduction ability and scarce active sites, which hinder the photocatalytic production of H2O2 by pure g-C3N5. Therefore, the photocatalytic activity of pure g-C3N5 in the generation of H2O2 is weak. Solving these limitations is a necessary condition for optimizing the efficiency of photocatalytic production of H2O2 using g-C3N5 materials. Researchers have deployed a series of strategies, including heterojunction formation, structural engineering, element doping, crystallinity regulation, etc. Among these methods, the construction of ultrathin nanosheet structures has emerged as a particularly effective way.
[0004] In order to solve the above problems and improve the photocatalytic activity of g-C3N5, the present invention designs a type of Na and K co-doped few-layer ultra-thin g-C3N5 photo-self-Fenton catalyst, and optimizes the morphology, structure and size of g-C3N5 by doping and crystallinity regulation, so that it becomes thinner and smaller. The synergistic effect of Na-K doping and crystallinity regulation can not only optimize the electronic structure and band structure of g-C3N5, so that the photocatalyst has a higher carrier separation efficiency, increase the density of active sites on the surface of g-C3N5, introduce functional groups and polar hydroxyl groups with higher oxygen content, but also improve the selectivity of ORR, efficiently produce H2O2, so as to realize the photo-self-Fenton of the catalyst; at the same time, effectively increase the electron mobility, so as to activate the n→π* electron transition, thereby effectively improving the photo-self-Fenton performance of g-C3N5, and efficiently degrade antibiotics in a short time, which is of great value for improving the added value of related products. Summary of the invention
[0005] In order to solve the problem of low H2O2 yield in existing g-C3N5 materials, the present invention provides a method for preparing a Na and K co-doped few-layer thin-sheet g-C3N5 photo-auto-Fenton catalyst, which specifically comprises the following steps:
[0006] (1) calcining dicyandiamide in a muffle furnace to obtain a precursor bulk carbon nitride (BCN), which is ground for later use;
[0007] (2) grinding and mixing carbon nitride (BCN), sodium chloride (NaCl) and potassium chloride (KCl), and then subjecting the mixture to secondary calcination in a muffle furnace to obtain a molten salt C3N5 ultrathin nanosheet;
[0008] (3) The obtained molten salt C3N5 ultrathin nanosheets are dispersed in pure water and heated and stirred, cooled and centrifuged to remove excess molten salt and other ions, and dried overnight to obtain Na-K co-doped few-layer thin sheet g-C3N5 photo-self-Fenton catalyst.
[0009] Preferably, the mass of dicyandiamide used in step (1) is 4.95-5.05 g.
[0010] Preferably, the calcination temperature of the muffle furnace in step (1) is 450-550° C., the heating rate is 8-12° C. / min, and the calcination time is 2-4 h.
[0011] Preferably, the grinding time in step (1) is 10 to 20 minutes.
[0012] Preferably, the mass ratio of carbon nitride (BCN), sodium chloride and potassium chloride in step (2) is (1.5-2.5):(4.5-5.5):(4.5-5.5), and the grinding time is 30-50 min.
[0013] Preferably, the calcination temperature of the muffle furnace in step (2) is 400-500° C., the heating rate is 8-12° C. / min, and the calcination time is 3-5 h.
[0014] Preferably, the heating temperature in step (3) is 80-120° C., the rotation speed is 600-800 r / min, and the heating time is 5-12 h.
[0015] Preferably, the washing method in step (3) is to thoroughly wash and separate with hot distilled water and anhydrous alcohol respectively, and dry at 70-90° C. overnight.
[0016] Preferably, the prepared Na-K co-doped few-layer thin flake g-C3N5 photo-self-Fenton catalyst is used to efficiently produce H2O2 in water.
[0017] Preferably, the prepared Na-K co-doped few-layer thin film g-C3N5 photo-self-Fenton catalyst acts in degrading tetracycline (TC) in water.
[0018] Beneficial effects of the present invention
[0019] (1) The present invention synthesizes Na-K co-doped few-layer thin flake g-C3N5 photo-auto-Fenton catalyst by doping and crystallinity regulation. Na-K co-doping makes g-C3N5 have more reactive sites, which can improve its utilization rate of photogenerated electrons, and provides a new idea for the preparation and functional optimization of g-C3N5 nanosheets and metal / non-metal doped composites under the synergistic effect of doping and crystallinity regulation.
[0020] (2) The present invention adopts the g-C3N5 photo-self-Fenton catalyst prepared by the synergistic method of doping and crystallinity regulation. Na-K co-doping optimizes the optical properties and surface structure of g-C3N5 nanosheets and reduces the resistance of charge transfer.
[0021] (3) The Na-K co-doped few-layer g-C3N5 photo-self-Fenton catalyst prepared by the present invention has smaller flakes and fewer layers accompanied by more delocalized electrons. Na-K co-doping can promote n→π* electron transition, which is beneficial to accelerate the separation efficiency and migration efficiency of photogenerated carriers and improve the charge density.
[0022] (4) Na-K co-doping can inhibit the recombination of photoinduced electron-hole pairs, increase the density of active sites on the g-C3N5 surface, and significantly improve the photo-Fenton performance of the g-C3N5 photo-Fenton catalyst.
[0023] (5) The Na-K co-doping of the g-C3N5 photo-Fenton catalyst in the present invention can effectively adjust the band gap of g-C3N5 to visible light and broaden its absorption range, thereby having higher visible light absorption capacity, enhanced light capture ability and excellent photocatalytic ability.
[0024] (6) The prepared Na-K co-doped CNAK photo-Fenton catalyst increased the density of active sites on the surface of g-C3N5, promoted the redox reaction, and had good photocatalytic activity, indicating that Na-K co-doping increased the photocatalytic activity of g-C3N5 to generate H2O2, and its H2O2 yield was 122.15 μmol g -1 h -1 , which is 11 times that of pure g-C3N5 (CNN) and 8-9 times that of the once calcined molten salt g-C3N5-Na-K (BCAK) catalyst.
[0025] (7) The equipment and materials required for the preparation method of the present invention are easy to obtain, the process operation is simple, and the process conditions are concise. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The XRD diagrams of the catalysts prepared in Example 1 and Comparative Examples 1 to 3 are shown.
[0027] Figure 2 These are SEM images of the catalysts prepared in Example 1 and Comparative Examples 1 to 3.
[0028] Figure 3 The corresponding AFM height images of the catalysts prepared in Example 1 and Comparative Example 3.
[0029] Figure 4 The UV-vis spectra of the catalysts prepared in Example 1 and Comparative Examples 1 to 3 are shown.
[0030] Figure 5 PL spectra of the catalysts prepared in Example 1 and Comparative Example 3.
[0031] Figure 6 EPR spectra of the catalysts prepared in Example 1 and Comparative Examples 1 to 3.
[0032] Figure 7 This is a comparison chart of the H2O2 production performance of the catalysts prepared in Example 1 and Comparative Examples 1 to 3.
[0033] Figure 8 This is the performance cycle diagram of the catalyst prepared in Example 1 for producing H2O2.
[0034] Fig. 9 The figure is a comparison chart of the degradation performance of catalysts prepared in Example 1 and Comparative Examples 1 to 3 on TC. DETAILED DESCRIPTION
[0035] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0036] Example 1
[0037] A Na and K co-doped few-layer g-C3N5 photo-auto-Fenton catalyst and a preparation method thereof, comprising the following steps:
[0038] (1) Preparation of precursor bulk BCN: 5 g of dicyandiamide was heated in a muffle furnace at 10 °C min -1 The temperature was raised to 500 °C and calcined for 3 h, followed by grinding in agate mortar for 15 min.
[0039] (2) 0.5 g of BCN, 1.25 g of NaCl, and 1.25 g of KCl were mixed and ground in agate mortar for 30 minutes to make them uniformly mixed, and then calcined in a muffle furnace at 10 °C min -1 The heating rate was increased to 450℃ and calcined for 4h.
[0040] (3) After the obtained mixture was naturally cooled to room temperature, it was thoroughly washed three times with distilled water and anhydrous alcohol respectively, and then filtered and separated to remove other ions. After being dried at 80°C for 12 h, the Na-K co-doped few-layer thin flake g-C3N5 photo-auto-Fenton catalyst (CNAK) was obtained.
[0041] Comparative Example 1
[0042] In comparison, the difference between this comparative example and Example 1 is that only K is doped in this comparative example to prepare a g-C3N5-K (CNK) catalyst, comprising the following steps:
[0043] (1) Preparation of precursor bulk BCN: 5 g of dicyandiamide was heated in a muffle furnace at 10 °C min -1 The temperature was raised to 500 °C and calcined for 3 h, followed by grinding in agate mortar for 15 min.
[0044] (2) 0.5 g BCN and 2.5 g KCl were mixed and ground in agate mortar for 30 minutes to make them uniformly mixed, and then calcined in a muffle furnace at 10 °C min -1 The heating rate was increased to 450℃ and calcined for 4h.
[0045] (3) After the obtained mixture was naturally cooled to room temperature, it was thoroughly washed three times with distilled water and anhydrous alcohol respectively, and then filtered and separated to remove other ions. After being dried at 80° C. for 12 h, the g-C3N5-K catalyst was collected.
[0046] Comparative Example 2
[0047] In contrast, the difference between this comparative example and Example 1 is that only Na is doped in this comparative example to prepare a g-C3N5-Na (CNA) catalyst, comprising the following steps:
[0048] (1) Preparation of precursor bulk BCN: 5 g of dicyandiamide was heated in a muffle furnace at 10 °C min -1 The temperature was raised to 500 °C and calcined for 3 h, followed by grinding in agate mortar for 15 min.
[0049] (2) 0.5 g of BCN and 2.5 g of NaCl were mixed and ground in agate mortar for 30 minutes to make them uniformly mixed, and then calcined in a muffle furnace at 10 °C min -1 The heating rate was increased to 450℃ and calcined for 4h.
[0050] (3) After the obtained mixture was naturally cooled to room temperature, it was thoroughly washed three times with distilled water and anhydrous alcohol respectively, and then filtered and separated to remove other ions. After being dried at 80°C for 12 h, the g-C3N5-K nanosheet catalyst was collected.
[0051] Comparative Example 3
[0052] In contrast, the present comparative example is different from Example 1 in that Na and K are not doped, and a g-C3N5 (CNN) nanosheet catalyst is prepared, comprising the following steps:
[0053] (1) Preparation of precursor bulk BCN: 5 g of dicyandiamide was heated in a muffle furnace at 10 °C min -1 The temperature was raised to 500 °C and calcined for 3 h, followed by grinding in agate mortar for 15 min.
[0054] (2) 0.5 g of BCN was placed in a muffle furnace for secondary calcination at 10 °C min -1 The temperature was raised to 450 °C and calcined for 4 h. After cooling to room temperature, the g-C3N5 catalyst was collected.
[0055] Comparative Example 4
[0056] In contrast, the difference between this comparative example and Example 1 is that only one calcination is performed to prepare a g-C3N5-Na-K (BCAK) catalyst, comprising the following steps:
[0057] 5 g of dicyandiamide, 1.25 g of NaCl and 1.25 g of KCl were heated in a muffle furnace at 10 °C min -1 The temperature was raised to 500 °C and calcined for 3 h. The mixture was ground in agate mortar for 15 min to obtain g-C3N5-Na-K (BCAK) catalyst.
[0058] Figure 1 X-ray diffraction experiments (XRD) of the precursor, the co-catalyst prepared in Example 1, and the catalysts prepared in Comparative Examples 1 to 3. It can be seen from the figure that the CNAK catalyst prepared in Example 1 not only has the characteristic peaks of g-C3N5, but also no new diffraction peaks related to K and Na elements are detected, which indicates that the molten salt modification does not change the lattice structure of g-C3N5, confirming the construction of the CNAK composite material.
[0059] Figure 2 The scanning electron microscope (SEM) of the co-doped catalyst prepared in Example 1 and the catalysts of Comparative Examples 1 to 3. It can be seen from the figure that compared with the g-C3N5 nanosheets (CNN) prepared in Comparative Example 3 ( Figure 2 (d)), CNK prepared in Comparative Example 1 ( Figure 2 (b)), in the CNA prepared in Comparative Example 2 ( Figure 2 (c) Na and K co-doped g-C3N5 nanosheets (CNAK) were further reduced by crystallinity control method ( Figure 2 (a)), indicating that CNAK photo-Fenton catalyst was successfully synthesized.
[0060] Figure 3 The corresponding height images of the co-doped catalyst prepared in Example 1 and the CNN catalyst prepared in Comparative Example 3 are obtained by atomic force microscopy (AFM). Figure 3 (A) and Figure 3 (B) shows that the CNN nanosheets of comparative example 3 and Figure 3 (C) and Figure 3 The relative heights of the CNAK ultrathin nanosheets of Example 1 in (D) are 16.3 nm and 3.55 nm (about 4 CN layers), respectively, indicating that they become thinner through the synergistic effect of doping and crystallinity regulation, and the morphology and size regulation of the CNAK photo-Fenton catalyst are successful.
[0061] Figure 4The UV-visible absorption (UV-vis) spectra of the catalyst prepared in Example 1 and the catalyst prepared in Comparative Examples 1 to 3 were used to test the light capture ability. It can be seen from the figure that the absorption edge of CNN in Comparative Example 3 is located at 388nm, while the absorption edge of CNAK in Example 1 shows an obvious red shift, and the absorption intensity in the visible light region is significantly enhanced, indicating that doping with Na-K can effectively adjust the band gap of CNN to visible light, broaden its absorption range, and is conducive to enhancing the ability of n→π* transition and light capture ability. The combination of doping and crystallinity regulation can synergistically promote n→π* electronic transition and improve visible light catalytic activity.
[0062] Figure 5 The photoluminescence (PL) spectra of the CNAK catalyst of Example 1 and the CNN of Comparative Example 3. Compared with the CNN catalyst, the PL intensity of the CNAK light from the Fenton catalyst is the weakest, showing a significant red shift, which may be caused by the expansion of the electronic conjugated system. CNAK shows only one emission peak in the PL spectrum, which originates from the →π* transition in the conjugated system, indicating that its charge pair transfer and separation effect is the best.
[0063] Figure 6 The electron paramagnetic resonance (EPR) spectra of the precursor BCN, the CNAK catalyst of Example 1, and the CNN catalyst of Comparative Example 3 can also indirectly confirm the occurrence of n→π* transition. As can be seen from the figure, the prepared material shows a clear Lorentzian line centered at a g value of 2.0052, which is related to the unpaired electrons in the conjugated aromatic ring. Relevant literature reports that n→π* electronic transitions excite more non-bonded electrons in the catalyst. Compared with CNN, CNAK exhibits a larger EPR enhancement signal span, indicating the presence of more unpaired electrons with n→π* electronic transitions.
[0064] H2O2 production experiment
[0065] The catalyst obtained in Example 1 and the catalysts obtained in Comparative Examples 1 to 3 were subjected to H2O2 production experiments, and the specific steps were as follows:
[0066] (1) Disperse 25 mg of the catalyst in a mixed aqueous solution of 30 mL of deionized water and 3 mL of ethanol.
[0067] (2) The reaction solution was placed under a simulated sunlight source using a 10W white light LED lamp to start the photoreaction test. 3 mL of the solution was extracted every 30 min, filtered through a 0.45 μm microfiltration membrane to remove the catalyst, and the H2O2 concentration was further analyzed.
[0068] (3) The iodine titration method is used to test the production of H2O2. 0.05 mL of 0.01 mol L -1Ammonium molybdate hydrate (H 32 Mo7N6O 28 ) solution and 2 mL of 0.1 mol L -1 The potassium iodide (KI) solution was allowed to stand for 5 min and then analyzed using a 350 nm UV-visible spectrum.
[0069] Figure 7 The results show that compared with CNN, the Na-K co-doped CNAK photo-Fenton catalyst has a higher yield, and the highest H2O2 yield of the CNAK catalyst is 122.15 μmol g -1 h -1 , which is 11 times the H2O2 yield of CNN catalyst.
[0070] Figure 8 This is a H2O2 production cycle experiment of the CNAK photo-Fenton catalyst prepared in Example 1. The figure shows that the CNAK catalyst has good stability.
[0071] Photo-Fenton degradation experiment
[0072] The CNAK photo-Fenton catalyst obtained in Example 1 and the catalysts obtained in Comparative Examples 1 to 3 were used for photo-Fenton degradation of antibiotics, and the specific steps were as follows:
[0073] (1) Weigh 20 mg of CNAK photo-Fenton catalyst and CNN catalyst respectively, disperse them into 50 mL of antibiotic aqueous solution (antibiotic concentration is 10 mg / L), stir for 30 min in dark conditions, and use appropriate ultrasonic dispersion to achieve adsorption-desorption equilibrium.
[0074] (2) Simulate the sunlight source by irradiating a white light LED lamp with an energy intensity of 10 W to initiate the photo-auto-Fenton reaction.
[0075] (3) Take 5 mL of solution every 30 minutes and use UV-visible spectrophotometer (UV-1800PC) to measure the absorbance of antibiotics. Tetracycline (TC) is measured at λ = 357 nm. The concentration of antibiotics is further calculated based on the standard curve of absorbance and concentration. The results are as follows: Figure 7 shown.
[0076] from Fig. 9 It can be seen that within 10 minutes, the removal rate of TC by the CNN sample of comparative example 3 is only 24.43%, while the removal rate of TC by the Na-K co-doped CNAK photo-Fenton catalyst in Example 1 is as high as 97.45%. The Na-K co-doping and crystallinity regulation method can improve the photo-Fenton activity of g-C3N5.
[0077] Compared with Comparative Example 3, the effect of the once-calcined BNAK prepared in Comparative Example 4 is improved to a certain extent; however, compared with the twice-calcined CNAK, the BNAK nanosheets are thicker, have fewer Na-K doping sites, and have lower photocatalytic activity, resulting in worse degradation performance and lower H2O2 yield.
[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and without departing from the spirit and scope of the technical solution of the present invention, which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a Na and K co-doped g-C3N5 photocatalyst, characterized in that: The following steps are involved: (1) calcining dicyandiamide in a muffle furnace to obtain a precursor bulk carbon nitride, which is ground for later use; (2) grinding and mixing carbon nitride, sodium chloride and potassium chloride, and then subjecting the mixture to secondary calcination in a muffle furnace to obtain a molten salt C3N5 ultrathin nanosheet; (3) The obtained molten salt C3N5 ultrathin nanosheets are dispersed in pure water and heated and stirred, cooled and centrifuged for washing, and dried overnight to obtain Na-K co-doped few-layer thin sheet g-C3N5 photo-self-Fenton catalyst.
2. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The mass of dicyandiamide used in step (1) is 4.95-5.05 g.
3. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The calcination temperature of the muffle furnace in step (1) is 450-550° C., the heating rate is 8-12° C. / min, and the calcination time is 2-4 hours.
4. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The grinding time in step (1) is 10 to 20 minutes.
5. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The mass ratio of carbon nitride (BCN), sodium chloride and potassium chloride in step (2) is (1.5-2.5):(4.5-5.5):(4.5-5.5), and the grinding time is 30-50 min.
6. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The calcination temperature of the muffle furnace in step (2) is 400-500° C., the heating rate is 8-12° C. / min, and the calcination time is 3-5 h.
7. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The heating temperature in step (3) is 80-120° C., the rotation speed is 600-800 r / min, and the heating time is 5-12 h.
8. The method for preparing the Na-K co-doped g-C3N5 photocatalyst according to claim 1, characterized in that: The washing method in step (3) is to thoroughly wash and separate with hot distilled water and anhydrous alcohol respectively, and dry at 70-90° C. overnight.
9. Use of the Na-K co-doped few-layer g-C3N5 photo-auto-Fenton catalyst prepared by the method of any one of claims 1 to 8 to produce hydrogen peroxide in water.
10. The role of the Na-K co-doped few-layer g-C3N5 photo-self-Fenton catalyst prepared by the method of any one of claims 1 to 8 in the degradation of tetracycline in water.
Citation Information
Patent Citations
Preparation of B-doped porous g-C3N4 catalyst and water treatment method based on catalyst
CN116196960A
Photocatalytic self-Fenton water treatment method based on S and K co-doped g-C3N4 nanosheet
CN117046500A
Preparation method and application of fused salt mediated CeO2 / Bi4TaO8Cl heterojunction catalyst
CN117943068A
Cited By
Homogeneous-heterogeneous double-junction coupled photocatalyst as well as preparation method and application thereof
CN120022925A
Modified nitrogen-rich carbon nitride as well as preparation method and photocatalytic application thereof
CN121178205A