Hyperbranched polyimide flexible foam and preparation method thereof

By using the preparation method of hyperbranched polyimide flexible foam with monoacid and single fat structure, the existing polyimide foam has solved the problems of high slag drop rate, low strength and uneven bubble cells during the foaming process, and achieved the The controllability of foam density and cell size improves the strength and product quality of the foam, and is suitable for applications in the fields of aviation, aerospace and ships.

CN119060336AActive Publication Date: 2024-12-03ZIGONG ZHONGTIANSHENG NEW MATERIAL TECH CO LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202411422439.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-03
Estimated Expiration
2044-10-12

AI Technical Summary

Technical Problem

The existing polyimide foam has problems such as high slag drop rate, low strength, uneven cell and high density during the foaming process, which limits its application in the fields of aviation, aerospace and ships.

Method used

The preparation method of hyperbranched polyimide flexible foam with mono-acid mono-lipid structure is adopted. The mono-acid mono-lipid mixture is formed by reflux reaction of different bifunctional aromatic dianhydrides with alcohol solvents and ether solvents, and the polyfunctional isocyanate is added. Then, gas volatilization is carried out under mechanical stirring and microwave, followed by adding foam stabilizer and deionized water, and foam molding is carried out by step heating or microwave curing.

Benefits of technology

The controllability of foam density and cell size is achieved, the strength of the foam and product quality are improved, the slag drop rate is reduced, the needs of industrial production are met, and the performance of the material is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060336A_ABST
    Figure CN119060336A_ABST
Patent Text Reader

Abstract

The invention relates to hyperbranched polyimide flexible foam and a preparation method thereof, and the method comprises the following steps: step 01, sequentially mixing a first bifunctional aromatic dianhydride, an alcohol solvent, an ether solvent and a polar organic solvent, and carrying out a reflux stirring reaction to obtain a first single-acid and single-ester mixed solution; 02, sequentially mixing a second bifunctional aromatic dianhydride, an alcohol solvent, an ether solvent, a ring-opening catalyst and a polar organic solvent, and carrying out reflux stirring reaction to obtain a second monoacid monoester mixed solution; step 03, mixing the first single-acid and single-ester mixed solution obtained in the step 01 and the second single-acid and single-ester mixed solution obtained in the step 02, adding polyfunctional isocyanate, and stirring until gas is volatilized; step 04, adding a foam stabilizer and deionized water into the mixed solution obtained in the step 03, and stirring; and step 05, injecting air into the mixed solution obtained in the step 04 to obtain the hyperbranched polyimide flexible foam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a hyperbranched polyimide flexible foam and a preparation method thereof. Background Art

[0002] Polyimide foam (PI) is a foam material made by polymerization and foaming reaction of polyimide resin raw materials with foaming agents, fillers and other additives. The polyimide foam molecular chain contains an imide ring, and the imide ring structure contains heterocyclic rings of nitrogen and oxygen atoms. The unique rigid imide ring molecular structure gives it good thermal oxidation resistance, insulation, radiation resistance and low temperature resistance. High-performance polyimide foam can even withstand extremely low temperatures and has the advantage of not breaking at -267°C. It is widely used in aerospace, aviation, engineering materials and other fields, and has also promoted the rapid development of the polyimide foam industry.

[0003] Chinese patent CN118005987A discloses a method for preparing polymethacrylimide foam (PMI). Methacrylic acid, 1-aminooctadecane, allyl methacrylate, tridecyl methacrylate, initiator, foaming agent and solvent are mixed and stirred for polymerization to prepare a copolymer plate, which is then heated and dried in a stepwise manner to obtain polymethacrylimide foam (PMI). This method for preparing polyimide foam is a commonly used polyimide preparation process in the industry. The imide structure is generated by rearrangement and cyclization between cyano and carboxyl molecules; in addition, the -CN in the MAN segment can also be rearranged to form a trapezoidal structure. Therefore, although the foam has high strength and good high temperature resistance, it can be used as a substitute for steel materials in various industries, but at the same time, it is rigid and easy to break, and the foam density is high, which greatly limits its application in ships, aerospace and other fields.

[0004] WO2004072032A2, US Pat. No. 6956066B2, US Pat. No. 7541388, US Pat. No. 2006063848 and Chinese Patent No. CN114854009A disclose a method for preparing a diacid diester precursor solution by reacting dianhydride, alcohol, catalyst, cross-linking agent, auxiliary material and solvent, and then adding isocyanate to the precursor solution for foaming to prepare polyimide foam. The polyimide foam prepared by the method has good comprehensive performance, but the foam has serious slag, low tensile strength, and gas is generated quickly and spontaneously after adding isocyanate during the processing, so it is difficult to stir evenly, the foaming process is difficult to control, and the yield of the foamed product is low.

[0005] U.S. Patents US4804504, US4814357, US4855332, US4952611, US5064867 and Chinese Patent CN114044903A disclose a method for preparing rigid polyimide foam. It uses anhydride, norbornene, polar solvent, catalyst and aromatic diamine as raw materials to react to generate polyester ammonium salt (PEAS), and then heats and foams to prepare polyimide foam. Although the polyimide foam is resistant to high temperatures, has good toughness, has small compression deformation at high temperatures, and can be recycled, the process is complicated, and the polyimide chain segments in the foam are one-dimensional linear structures without three-dimensional network crosslinking, which makes the product low in strength and high-temperature resistance, and difficult to use for a long time in a complex environment of high temperature and high strength.

[0006] At present, the preparation of polyimide foam adopts the self-foaming method, but there are still problems such as excessive foaming process, serious cell collapse and low yield rate. Therefore, it is urgent to prepare a polyimide flexible foam with low density, uniform cells, qualified strength and low slag rate, which can be used as a weight-reducing, heat-insulating and flame-retardant material in the fields of aviation, aerospace and ships. Summary of the invention

[0007] The present invention provides a hyperbranched polyimide flexible foam and a preparation method thereof to solve the above-mentioned deficiencies in the prior art. The polyimide foam intermediate prepared by the present invention has a monoacid monoester structure rather than a diacid diester structure, which can improve the quality problems of high slag drop rate and low strength of foam products.

[0008] In order to achieve the purpose of the present invention, the following technologies are proposed: A hyperbranched polyimide flexible foam, the chemical structure of which is in, R1 is selected from: .

[0009] A method for preparing a hyperbranched polyimide flexible foam comprises the following steps: Step 01, sequentially mixing a first difunctional aromatic dianhydride, an alcohol solvent, an ether solvent, and a polar organic solvent, and reacting by reflux stirring to obtain a first monoacid monolipid mixed solution, wherein the reaction temperature is about 55° C., and the reaction time is 10-16 hours; Step 02, sequentially mixing the second difunctional aromatic dianhydride, alcohol solvent, ether solvent, ring-opening catalyst, and polar organic solvent, and reacting by reflux stirring to obtain the second monoacid monolipid mixed solution, the reaction temperature is about 55° C., and the reaction time is 10-16 hours; Step 03, mixing the first monoacid monoester mixed solution obtained in step 01 and the second monoacid monoester mixed solution obtained in step 02, adding multifunctional isocyanate, and stirring until the gas is volatilized; Step 04, adding a foam stabilizer and deionized water to the mixed solution obtained in step 03, and mechanically stirring the mixture at a speed of 1000-1500 r / min for 1-2 hours, and then stirring the mixture by microwave stirring at 20 kHz for 1-2 hours; Step 05, injecting air into the mixed solution obtained in step 04 at a rate of 0.5-1NL / min, and then injecting the mixed solution into a mold and foaming it in a stepwise heating or microwave curing manner at 60°C for 4 hours, 150°C for 4 hours, and 220°C for 4 hours to obtain a hyperbranched polyimide flexible foam.

[0010] Further, the chemical structural formula of the monoacid monolipid is Wherein, R1 is selected from: The mono-acid mono-fat mixed liquid can be one or a mixture of more than one of the mono-acid mono-fat, and each mono-acid mono-fat mixed liquid is prepared separately.

[0011] Furthermore, the first difunctional aromatic dianhydride and the second difunctional aromatic dianhydride are one or more monomers of dianhydride groups such as 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride), 3,3',4,4'-triphenylbisether tetracarboxylic dianhydride, and 3,3',4,4'-tetracarboxylic diphenyl ether dianhydride.

[0012] Furthermore, the alcohol solvent is one or more alcohols such as methanol, ethanol, propanol, furfuryl alcohol, etc., and the mass ratio of the alcohol solvent to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride is 1:1. When the alcohol solvent is excessive, esterification is performed to form diacid diesters.

[0013] Furthermore, the ether solvent is tetrahydrofuran, and the mass of the ether solvent is 4-6 times that of the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride. When the ether solvent is used in excess, the surface tension of the system can be reduced, thereby facilitating the release of gas.

[0014] Furthermore, the polar organic solvent is one or more of ethyl acetate, dichloromethane, acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.

[0015] Furthermore, the foam stabilizer is one or more of AK-8805, AK-158, DC-193, DC-198, L550, L6900, AK-8803, L550, AK-168, octadecyl dimethyl amine oxide, MQ803 and other auxiliary agents, and the mass ratio of the foam stabilizer to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride is 0.5-2:100.

[0016] Furthermore, the multifunctional isocyanate is one or more of PM-200, PM-400, PM-2010, PM-130, polymethylene polyphenyl polyisocyanate, and the mass ratio of isocyanate groups in the multifunctional isocyanate to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride is 99:50.

[0017] Furthermore, the ring-opening catalyst is one or more of dimethylimidazole and isoquinoline, and the mass ratio of the ring-opening catalyst to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride is 0.5-2:100.

[0018] The advantages of the above technical solution are: The present invention uses different difunctional aromatic dianhydrides to be dissolved in alcohol solvents, ether solvents and catalysts, and refluxes at high temperature to generate a monoacid and monolipid mixed liquid, and then adds a multifunctional isocyanate. After the system spontaneously generates gas CO2 and completely volatilizes, a foam stabilizer, a foaming agent and the like are added, stirred evenly, and the temperature is increased in a stepwise manner for foaming to obtain a hyperbranched polyimide flexible foam material.

[0019] The polyimide foam prepared by the present invention is end-capped with anhydride groups, which can improve the physical and mechanical properties of foam products. In addition, according to previous experiments, it is known that the foam products prepared by directly esterifying the difunctional aromatic dianhydride to diacid diester have a high slag rate and low strength, while the quality problem can be solved by esterifying the difunctional aromatic dianhydride to monoacid monoester and then preparing the foam. Because the active electron affinity (Ea) of different difunctional aromatic dianhydrides is different, and it is difficult to ensure that the reaction degree of each difunctional aromatic dianhydride is consistent during the reaction, the A material is prepared by first esterifying it separately to monoacid monoester and then stirring and mixing it according to the use requirements. Under the original process, after adding isocyanate, the mixed liquid reacts rapidly and violently to produce bubbles, which can easily lead to large-scale collapse of the foam, the bubble size is difficult to control, and the stirring processing time is insufficient and the mixing is uneven, resulting in a series of product quality problems.

[0020] The present invention does not use the self-generated gas CO2 of the system for foaming. By reducing the surface tension of the system, the bubbles generated by the self-generated gas CO2 of the system are completely broken. After the gas evaporates, a foam stabilizer and water are added, and then the mixture is stirred evenly under the combined action of long-term mechanical stirring and ultrasonic stirring. The preparation of the hyperbranched polyimide flexible foam is completed by continuous foaming and imidization in a step-by-step heating manner.

[0021] The hyperbranched polyimide flexible foam prepared by the invention has controllable foam density and pore size, stable foam product quality and uniform pores, and can meet the needs of continuous large-scale industrial production.

[0022] The present invention injects a small amount of air into the foaming system, and can form a large number of micro-bubble nuclei inside the polyimide under the action of high-speed stirring, so that the foam pores of the polyimide foam during the foaming process are more uniform and delicate, and not easy to fall off, thereby enhancing product performance and meeting the needs of continuous large-scale industrial production.

[0023] The hyperbranched polyimide flexible foam prepared by the present invention can be supplemented with fillers such as flame retardant, glass fiber, carbon fiber, wollastonite and absorbent when adding a foam stabilizer according to the application to enhance the performance of the foam material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.

[0025] Figure 1 The infrared spectrum of the hyperbranched polyimide flexible foam material after imidization is shown.

[0026] Figure 2 A physical picture of the hyperbranched polyimide flexible foam prepared in Example 1 is shown.

[0027] Figure 3 A physical picture of the hyperbranched polyimide flexible foam prepared in Comparative Example 2 is shown.

[0028] Figure 4 A cross-sectional view of the hyperbranched polyimide flexible foam prepared in Comparative Example 2 is shown. DETAILED DESCRIPTION

[0029] In order to verify the foam synthesis effect, foam was prepared by the so-called preparation method and infrared spectrum test was carried out. Figure 1 The infrared spectrum of the hyperbranched polyimide flexible foam material after imidization is shown in the figure. Combined with the infrared characteristic absorption peak analysis of the main chemical groups in the "Chemistry and Chemical Engineering Experimenter's Manual", it can be seen that 1371.14cm -1It should be the stretching vibration peak of CN, 1778.00cm -1 and 1719.41cm -1 They are the asymmetric stretching vibration absorption peak and the symmetric stretching vibration absorption peak of C=O, 1371.14 cm -1 and 722.06cm -1 They are the characteristic absorption peaks of the stretching and bending vibrations of the CNC bonds on the imide ring.

[0030] Example 1 Step 01, add 322.2g of 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 46.0g of ethanol, 1288.8g of tetrahydrofuran, 322.2g of N,N-dimethylformamide, and 3.2g of dimethylimidazole to a flask in sequence, reflux and stir to react at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain the first mono-acid mono-fat mixed solution.

[0031] Step 02, add 310.2 g of 3,3',4,4'-tetracarboxylic acid diphenyl ether dianhydride, 46.0 g of ethanol, 1240.8 g of tetrahydrofuran, 310.2 g of N,N-dimethylformamide, and 3.2 g of dimethylimidazole to the flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain a second mono-acid mono-fat mixed solution.

[0032] Step 03, mix the first monoacid and monofat mixed liquid and the second monoacid and monofat mixed liquid, add 554.4g of polyphenyl polymethylene polyisocyanate, continue stirring until the gas is completely volatilized, add 6.3g of AK-8805 and 63g of deionized water, and use mechanical stirring to continue stirring at 1000r / min for 2h, and then stir by microwave at 20kHz for 2h.

[0033] Step 04, injecting a small amount of air into the mixed liquid at a speed of 0.8NL / min, transferring the mixed liquid to a mold and free foaming molding at 60℃×4h, 150℃×4h, and 220℃×4h in sequence to obtain a hyperbranched polyimide flexible foam.

[0034] Example 2 Step 01, add 322.2g of 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 46.0g of ethanol, 1288.8g of tetrahydrofuran, 322.2g of N,N-dimethylformamide, and 6.3g of dimethylimidazole to a flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain the first mono-acid mono-fat mixed solution.

[0035] Step 02, add 310.2 g of 3,3',4,4'-tetracarboxylic acid diphenyl ether dianhydride, 46.0 g of ethanol, 1240.8 g of tetrahydrofuran, 310.2 g of N,N-dimethylformamide, and 3.1 g of dimethylimidazole to the flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain a second mono-acid mono-fat mixed solution.

[0036] Step 03, add 218.1 g of pyromellitic anhydride, 46.0 g of ethanol, 872.4 g of tetrahydrofuran, 218.1 g of N,N-dimethylformamide, and 2.1 g of dimethylimidazole to the flask in sequence, reflux and stir to react at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain the third mono-acid and mono-fat mixed solution.

[0037] Step 04, mix the first monoacid monofat mixture, the second monoacid monofat mixture and the third monoacid monofat mixture, add 831.6g of polyphenyl polymethylene polyisocyanate, continue stirring until the gas is completely volatilized, add 9.4g of AK-8805 and 94g of deionized water, and use mechanical stirring at 1000r / min for 2h, and then stir by microwave at 20kHz for 2h.

[0038] Step 05, inject a small amount of air into the mixed liquid at a speed of 0.8NL / min, transfer the mixed liquid to a mold and free foaming it at 60℃×4h, 150℃×4h, and 220℃×4h in sequence to obtain a hyperbranched polyimide flexible foam.

[0039] Example 3 Step 01, add 436.2g of pyromellitic anhydride, 92.0g of ethanol, 1744.8g of tetrahydrofuran, 436.2g of N,N-dimethylformamide, and 4.3g of dimethylimidazole to the flask in sequence, reflux and stir to react at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain the first mono-acid and mono-fat mixed solution.

[0040] Step 02, add 554.4g of polyphenyl polymethylene polyisocyanate to the monoacid and monofat mixture, continue stirring until the gas is completely volatilized, then add 4.3g of AK-8805 and 43g of deionized water, and use mechanical stirring to continue stirring at 1000r / min for 2h, and then stir by microwave at 20kHz for 2h.

[0041] Step 03, inject a small amount of air into the mixed liquid at a speed of 0.8NL / min, transfer the mixed liquid to a mold and free foaming it at 60℃×4h, 150℃×4h, and 220℃×4h in sequence to obtain a hyperbranched polyimide flexible foam.

[0042] Comparative Example 1 Step 01, add 322.2g of 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 92.0g of ethanol, 1288.8g of tetrahydrofuran, 322.2g of N,N-dimethylformamide, and 6.3g of dimethylimidazole to a flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain the first mono-acid mono-fat mixed solution.

[0043] Step 02, add 310.2 g of 3,3',4,4'-tetracarboxylic acid diphenyl ether dianhydride, 92.0 g of ethanol, 1240.8 g of tetrahydrofuran, 310.2 g of N,N-dimethylformamide, and 6.3 g of dimethylimidazole to the flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain a second mono-acid mono-fat mixed solution.

[0044] Step 03, mix the first monoacid and monofat mixed liquid and the second monoacid and monofat mixed liquid, add 554.4g of polyphenyl polymethylene polyisocyanate, continue stirring until the gas is completely volatilized, add 6.3g of AK-8805 and 63g of deionized water, and use mechanical stirring to continue stirring at 1000r / min for 2h, and then stir by microwave at 20kHz for 2h.

[0045] Step 04, inject a small amount of air into the mixed liquid at a speed of 0.8NL / min, transfer the mixed liquid to a mold and free foaming it at 60℃×4h, 150℃×4h, and 220℃×4h in sequence to obtain polyimide flexible foam.

[0046] Comparative Example 2 Step 01, add 322.2g of 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 92.0g of ethanol, 644.4g of tetrahydrofuran, 322.2g of N,N-dimethylformamide, and 6.3g of dimethylimidazole to a flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain the first mono-acid mono-fat mixed solution.

[0047] Step 02, add 310.2 g of 3,3',4,4'-tetracarboxylic acid diphenyl ether dianhydride, 92.0 g of ethanol, 644.4 g of tetrahydrofuran, 310.2 g of N,N-dimethylformamide, and 6.3 g of dimethylimidazole to the flask in sequence, reflux and stir at 55°C for 10 hours until the mixed solution becomes clear and transparent, to obtain a second mono-acid mono-fat mixed solution.

[0048] Step 03, mix the first monoacid monolipid mixed solution and the second monoacid monolipid mixed solution, add 6.3g AK-8805 and 554.4g polyphenyl polymethylene polyisocyanate in sequence, and continue to stir and foam. After the foaming is completed, heat and cure at 150℃×4h and 220℃×4h to obtain polyimide flexible foam.

[0049] In Comparative Example 1, compared with Example 1, the amount of alcohol solvent used is doubled, and all difunctional aromatic dianhydrides can be reacted into diacid diesters. Comparative Example 2 is based on Comparative Example 1, and the amount of ether solvent used is reduced. 2 Foam molding.

[0050] The performance of the hyperbranched polyimide flexible foam prepared in each embodiment and comparative example is shown in Table 1. In summary, combined with Figures 2 to 4 As shown in the above table, after changing the synthetic diacid diester to monoacid monofats, the mechanical strength of the foam is significantly improved, and the problem of foam falling off is basically solved; at the same time, after improving the foaming process, the foam pores are more uniform, the density is controllable, and no obvious collapse phenomenon is found.

[0051] For ships, weight reduction is equivalent to fuel saving or increased carrying capacity. The polyimide foam prepared by the present invention can be used as a substitute for traditional mineral wool materials for ships. Compared with the original solution, it can reduce the weight of ships and reduce energy demand while meeting the use requirements.

[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A hyperbranched polyimide flexible foam, characterized in that: Its chemical structure is in, R1 is selected from: 。 2. A method for preparing a hyperbranched polyimide flexible foam, characterized in that: Includes steps: Step 01, sequentially mixing a first difunctional aromatic dianhydride, an alcohol solvent, an ether solvent, and a polar organic solvent, and reacting by reflux stirring to obtain a first monoacid monolipid mixed solution, wherein the reaction temperature is about 55° C., and the reaction time is 10-16 hours; Step 02, sequentially mixing the second difunctional aromatic dianhydride, alcohol solvent, ether solvent, ring-opening catalyst, and polar organic solvent, and reacting by reflux stirring to obtain the second monoacid monolipid mixed solution, the reaction temperature is about 55° C., and the reaction time is 10-16 hours; Step 03, mixing the first monoacid monoester mixed solution obtained in step 01 and the second monoacid monoester mixed solution obtained in step 02, adding multifunctional isocyanate, and stirring until the gas is volatilized; Step 04, adding a foam stabilizer and deionized water to the mixed solution obtained in step 03, and mechanically stirring the mixture at a speed of 1000-1500 r / min for 1-2 hours, and then stirring the mixture by microwave stirring at 20 kHz for 1-2 hours; Step 05, injecting air into the mixed solution obtained in step 04 at a rate of 0.5-1NL / min, and then injecting the mixed solution into a mold and foaming it in a stepwise heating or microwave curing manner at 60°C for 4 hours, 150°C for 4 hours, and 220°C for 4 hours to obtain a hyperbranched polyimide flexible foam.

3. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The chemical structure of monoacid monolipid is Wherein, R1 is selected from: The mono-acid mono-fat mixed liquid can be one or a mixture of more than one of the mono-acid mono-fat, and each mono-acid mono-fat mixed liquid is prepared separately.

4. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The first difunctional aromatic dianhydride and the second difunctional aromatic dianhydride are one or more monomers of dianhydride groups such as 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride), 3,3',4,4'-triphenylbisether tetracarboxylic dianhydride, and 3,3',4,4'-tetracarboxylic diphenyl ether dianhydride.

5. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The alcohol solvent is one or more alcohols such as methanol, ethanol, propanol, furfuryl alcohol, etc., and the mass ratio of the alcohol solvent to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride is 1:

1.

6. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The ether solvent is tetrahydrofuran, and the mass of the ether solvent is 4-6 times that of the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride.

7. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The polar organic solvent is one or more of ethyl acetate, dichloromethane, acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

8. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The foam stabilizer is one or more of AK-8805, AK-158, DC-193, DC-198, L550, L6900, AK-8803, L550, AK-168, octadecyl dimethyl amine oxide, MQ803 and other auxiliary agents, and the mass ratio of the foam stabilizer to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride is 0.5-2:

100.

9. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The multifunctional isocyanate is one or more of PM-200, PM-400, PM-2010, PM-130, polymethylene polyphenyl polyisocyanate, and the mass ratio of isocyanate group to the first difunctional aromatic dianhydride or the second difunctional aromatic dianhydride in the multifunctional isocyanate is 99:

50.

10. The method for preparing a hyperbranched polyimide flexible foam according to claim 2, characterized in that: The ring-opening catalyst is one or more of dimethylimidazole and isoquinoline, and the mass ratio of the ring-opening catalyst to the first bifunctional aromatic dianhydride or the second bifunctional aromatic dianhydride is 0.5-2:100.

Citation Information

Patent Citations

  • Hard polyimide foam as well as preparation method and application thereof

    CN114044903A

  • Polyimide foam and preparation method thereof

    CN114854009A

  • Polymethacrylimide foam and preparation method thereof

    CN118005987A

  • Polyimide foams

    US20060063848A1

  • Production of foamed polymer structures

    US4804504A