Tin-bismuth alloy material for underground packing and preparation method of tin-bismuth alloy material
By adding antimony and silver to the tin bismuth alloy to refine the grains, the cracks, expansion and contraction and corrosion problems of traditional cement sealing materials in the downhole environment are solved, and the tin bismuth alloy with high mechanical strength and corrosion resistance is achieved. Materials, providing a low-cost, environmentally friendly permanent sealing solution.
Patent Information
- Application Number
- CN202411464527.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional cement sealing materials have problems such as cracks, expansion and contraction, and corrosion in the underground environment, resulting in unstable sealing effect and high cost, making it difficult to achieve environmentally friendly and low-cost permanent sealing.
A tin bismuth alloy material is used, and by adding antimony and silver to it, the grains are refined, and the mechanical properties and corrosion resistance are improved, a tin bismuth alloy material with excellent mechanical properties and sealing properties is prepared.
The high mechanical strength, low thermal expansion coefficient, thermal fatigue resistance and good corrosion resistance of tin bismuth alloy are achieved, which significantly improves the performance and reliability of downhole sealing materials and reduces costs.
Smart Images

Figure HDA0005092902040000011 
Figure HDA0005092902040000012 
Figure HDA0005092902040000021
Abstract
Description
Technical Field
[0001] The invention relates to a tin-bismuth alloy for downhole isolation and a preparation method thereof, which is applied to downhole isolation in oil fields and belongs to the technical field of oil and gas well plugging. Background Art
[0002] Plugging and abandoning wells is an inevitable part of the life cycle of oil wells. Once an oil well is exhausted or no longer has mining value, the abandoned well will be plugged and sealed to prevent greenhouse gases such as methane and other harmful substances from leaking into the environment, in order to protect the ecosystem and the health and safety of local people.
[0003] When plugging, it can be very time-consuming and therefore costly, depending on the well conditions. Traditionally, cement is usually used to plug abandoned wells, but this method is not reliable, especially when plugging offshore oil wells. Because cement shrinks during the curing process, it may cause cracks inside, reduce the integrity of the isolation layer, form a leakage path, and affect the isolation effect. When the temperature changes, the cement will expand and shrink, further affecting the isolation quality. In addition, cement has poor corrosion resistance and is sensitive to acidic water and salt water. Long-term exposure to this environment will cause corrosion and induce fluid migration. It takes a certain amount of time for cement to cure, usually several hours or even days to reach the designed strength, and the quality of cement depends largely on the quality of construction; when cement is cured, it can no longer be processed or adjusted, and it is difficult to monitor its performance and integrity in real time. Other types of alternative plugging materials and emerging plugging materials, such as blast furnace slag and resin, also have different disadvantages. When blast furnace slag is actually used, the solidified slag cement is prone to cracks. The strength of resin decreases in downhole environments, such as crude oil and H2S. Therefore, there is an urgent need for an environmentally friendly, lower-cost plugging material that can permanently abandon the well.
[0004] As a substitute for cement, bismuth-based alloys have been proposed for plugging and abandoning oil wells. Alloy seals are more advantageous than cement seals because they can significantly reduce the cost of well abandonment. As a low-melting-point alloy, the melting point of tin-bismuth alloy can be controlled to vary in the range of 95°C to 263°C, and no other Sn or Bi compounds will be formed. Due to the characteristics of bismuth, the alloy will expand in volume during solidification to form good sealing properties. In addition, tin-bismuth alloy has low thermal expansion coefficient, thermal fatigue resistance, high mechanical strength, pressure resistance and creep resistance, making it the most popular material in plugging and abandoning well applications in recent years. However, metal Bi is relatively brittle, which makes bismuth alloys more brittle, with poor ductility and plasticity, and brittle fracture may occur in severe cases. Summary of the invention
[0005] The purpose of the present invention is to provide a tin-bismuth alloy material and a preparation method thereof in view of the current domestic blank of low-melting-point alloy for downhole packers. The tin-bismuth alloy developed by the present invention has excellent mechanical properties, sealing properties, and corrosion resistance. By adding antimony and silver to the tin-bismuth alloy, the grains can be refined, the coarsening and brittleness of bismuth can be slowed down, the mechanical properties of the alloy can be improved, and the corrosion resistance of the alloy can be improved.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A tin-bismuth alloy material for underground isolation, wherein the mass composition percentage of the tin-bismuth alloy material is:
[0008] Bi 56-59wt%, Sb 0.1-1.0wt%, Ag 0.1-1.0wt%, and the balance is Sn. Preferably Bi 57wt%, Sb 0.5wt%, Ag 0.2wt%, and the balance is Sn.
[0009] The present invention provides a method for preparing a tin-bismuth alloy material for underground isolation, comprising the following steps:
[0010] (1) Weigh pure tin, pure bismuth, pure antimony and pure silver according to the above-mentioned content of Bi 56-59wt.%, Sb 0.1-1.0wt.%, Ag 0.1-1.0wt.%, and the balance being Sn, and remove the surface oxide scale;
[0011] (2) Put the pure tin, pure bismuth, pure antimony and pure silver in step (1) into a clean graphite crucible, and put them together into the furnace of a resistance furnace, and heat the resistance furnace to 600° C. During this smelting process, introduce argon protective gas, and after the metal is completely melted, keep it warm and stand for 20 to 30 minutes, and then stir it for 1 to 2 minutes;
[0012] The metal in step (2) is kept warm for 5 to 10 minutes, the scum on the surface of the melt is removed, the crucible is taken out and allowed to stand, and when the melt temperature drops to 300° C., the melt is poured into a graphite mold, and after solidification, it is naturally cooled to obtain an ingot.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] By adding a small amount of alloying elements Sb and Ag, the coarsening and brittleness of bismuth can be slowed down, the alloy structure can be refined, and the mechanical properties and corrosion resistance of the alloy can be improved. The addition of Sb can prevent the coarsening of the microstructure and improve the ductility of the alloy, and improve the corrosion resistance of the tin-bismuth alloy. The addition of Ag improves the strength and creep resistance of the tin-bismuth alloy and improves the comprehensive mechanical properties of the alloy. The present invention provides a tin-bismuth alloy material with good mechanical properties and excellent corrosion resistance through a traditional casting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The metallographic microscope photos of the tin-bismuth alloy materials of Example 3 of the present invention and Comparative Example 1 are shown.
[0016] Figure 2 The AC impedance curves of the tin-bismuth alloy of Example 3 of the present invention and Comparative Example 1 are shown.
[0017] Figure 3 The weight loss curves of the tin-bismuth alloy materials of Example 3 and Comparative Example 1 in the salt spray test of the present invention are shown. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below in conjunction with specific implementation schemes. It is pointed out that the following implementation cases are only used to illustrate the specific implementation methods of the present invention and cannot limit the scope of protection of the present invention.
[0019] Example 1
[0020] A tin-bismuth alloy material for underground isolation, wherein the mass composition percentage of the tin-bismuth alloy is: Bi 57wt.%, Sb 0.3wt.%, Ag 0.2wt.%, and the balance is Sn.
[0021] (1) According to the above content of Bi 57wt.%, Sb 0.3wt.%, Ag 0.2wt.%, and the balance being Sn in weight percentage, pure tin, pure bismuth, pure antimony, and pure silver are weighed, and the surface oxide scale is removed;
[0022] (2) Put the pure tin, pure bismuth, pure antimony and pure silver in step (1) into a clean graphite crucible, and put them together into the furnace of a resistance furnace, and heat the resistance furnace to 600° C. During this smelting process, introduce argon protective gas, and after the metal is completely melted, keep it warm and stand for 30 minutes, and then stir it for 2 minutes;
[0023] (3) The metal in step (2) is kept warm for 10 minutes, the scum on the surface of the melt is removed, the crucible is taken out and allowed to stand, and when the melt temperature drops to 300° C., the melt is poured into a graphite mold, and after solidification, it is naturally cooled to obtain an ingot.
[0024] Example 2
[0025] A tin-bismuth alloy material for underground isolation, wherein the mass composition percentage of the tin-bismuth alloy is: Bi 57wt.%, Sb 0.4wt.%, Ag 0.2wt.%, and the balance is Sn.
[0026] (1) According to the above content of Bi 57wt.%, Sb 0.4wt.%, Ag 0.2wt.%, and the balance being Sn in weight percentage, pure tin, pure bismuth, pure antimony, and pure silver are weighed, and the surface oxide scale is removed;
[0027] (2) Put the pure tin, pure bismuth, pure antimony and pure silver in step (1) into a clean graphite crucible, and put them together into the furnace of a resistance furnace, and heat the resistance furnace to 600° C. During this smelting process, introduce argon protective gas, and after the metal is completely melted, keep it warm and stand for 30 minutes, and then stir it for 2 minutes;
[0028] (3) The metal in step (2) is kept warm for 10 minutes, the scum on the surface of the melt is removed, the crucible is taken out and allowed to stand, and when the melt temperature drops to 300° C., the melt is poured into a graphite mold, and after solidification, it is naturally cooled to obtain an ingot.
[0029] Example 3
[0030] A tin-bismuth alloy material for underground isolation, wherein the mass composition percentage of the tin-bismuth alloy is: Bi 57wt.%, Sb 0.5wt.%, Ag 0.2wt.%, and the balance is Sn.
[0031] (1) According to the above content of Bi 57wt.%, Sb 0.5wt.%, Ag 0.2wt.%, and the balance being Sn in weight percentage, pure tin, pure bismuth, pure antimony, and pure silver are weighed, and the surface oxide scale is removed;
[0032] (2) Put the pure tin, pure bismuth, pure antimony and pure silver in step (1) into a clean graphite crucible, and put them together into the furnace of a resistance furnace, and heat the resistance furnace to 600° C. During this smelting process, introduce argon protective gas, and after the metal is completely melted, keep it warm and stand for 30 minutes, and then stir it for 2 minutes;
[0033] (3) The metal in step (2) is kept warm for 10 minutes, the scum on the surface of the melt is removed, the crucible is taken out and allowed to stand, and when the melt temperature drops to 300° C., the melt is poured into a graphite mold, and after solidification, it is naturally cooled to obtain an ingot.
[0034] Comparative Example 1
[0035] A conventional tin-bismuth alloy material, wherein the mass composition percentage of the tin-bismuth alloy is: Bi 57wt.%, and the balance is Sn.
[0036] (1) Weigh pure tin and pure bismuth according to the above content of Bi 57wt.%, and the balance is the weight percentage of Sn, and remove the surface oxide scale;
[0037] (2) Put the pure tin and pure bismuth in step (1) into a clean graphite crucible, and put them together into the furnace of a resistance furnace, and heat the resistance furnace to 300° C. During this smelting process, introduce argon protective gas, and after the metal is completely melted, keep it warm and let it stand for 30 minutes, and then stir it for 2 minutes;
[0038] (3) The metal in step (2) is kept warm for 10 minutes, the scum on the surface of the melt is removed, the crucible is taken out and the melt is poured into a graphite mold, and after solidification, it is naturally cooled to obtain an ingot.
[0039] By comparing the microstructures of the tin-bismuth alloy of Example 3 and Comparative Example 1, it can be seen that the microstructure of the tin-bismuth alloy of Example 3 after adding appropriate amounts of Sb and Ag elements is finer than that of the tin-bismuth alloy of Comparative Example 1. After hardness testing, tensile testing and compression testing, it was found that the tin-bismuth alloy of Example 3 has higher hardness, better tensile strength and yield strength than the tin-bismuth alloy of Comparative Example 1.
[0040] The salt spray corrosion test was performed on Example 3 and Comparative Example 1. Figure 3 It can be seen that the corrosion resistance of tin-bismuth alloy can be improved by adding appropriate amounts of Sb and Ag elements.
[0041] Electrochemical tests were performed on Example 3 and Comparative Example 1. Figure 2 It can be seen that Example 3 has a larger capacitive reactance arc, indicating that Example 3 has better corrosion resistance. After adding appropriate amounts of Sb and Ag elements, the corrosion resistance of the tin-bismuth alloy can be improved.
[0042] A sealing test was conducted on Example 3. The alloy was made into a 45 mm × 180 mm × 21.59 mm alloy sealing plug and combined with a casing to conduct air and liquid sealing tests. Under air pressure testing and hydraulic pressure testing, no sealing failure occurred within 240 hours, indicating that Example 3 has good sealing performance and can be used for downhole isolation in oil fields.
[0043] The invention reduces the coarsening and brittleness of bismuth by adding appropriate amounts of Sb and Ag elements, improves the mechanical properties and corrosion resistance of the tin-bismuth alloy, and the prepared tin-bismuth alloy material has good sealing performance.
[0044] Although the preferred experimental cases have been listed and described in detail here, those skilled in the art will appreciate that various improvements, additions, substitutions, etc. may be made without departing from the essence of the invention, and these contents are considered to be within the scope of the invention as defined by the patent requirements.
Claims
1. A tin-bismuth alloy material for underground isolation, characterized in that: The mass composition percentage of the tin-bismuth alloy material is: Bi 56-59wt.%, Sb 0.1-1.0wt.%, Ag 0.1-1.0wt.%, and the balance is Sn.
2. A tin-bismuth alloy material for underground isolation according to claim 1, characterized in that Sb 0.1~1.0wt.%, Ag 0.1~1.0wt.%.
3. A method for preparing the tin-bismuth alloy material for downhole isolation according to claim 1 or 2, characterized in that: The following steps are involved: (1) Weigh pure tin, pure bismuth, pure antimony and pure silver according to the above-mentioned content of Bi 56-59wt.%, Sb 0.1-1.0wt.%, Ag 0.1-1.0wt.%, and the balance being Sn, and remove the surface oxide scale; (2) Put the pure tin, pure bismuth, pure antimony and pure silver in step (1) into a clean graphite crucible, and put them together into the furnace of a resistance furnace, and heat the resistance furnace to 600° C. During this smelting process, introduce argon protective gas, and after the metal is completely melted, keep it warm and stand for 20 to 30 minutes, and then stir it for 1 to 2 minutes; (3) The metal in step (2) is kept warm for 5 to 10 minutes, the scum on the surface of the melt is removed, the crucible is taken out and allowed to stand, and when the melt temperature drops to 300° C., the melt is poured into a graphite mold, and after solidification, it is naturally cooled to obtain an ingot.
Citation Information
Cited By
Sn-Bi-Sb alloy for oil well plugging as well as preparation method and application of Sn-Bi-Sb alloy
CN121951308A