Method for preparing ethylene through acetylene electroreduction and removing impurities of acetylene in ethylene-acetylene mixed gas by using binuclear copper molecular catalyst

By using a binuclear copper molecular catalyst in electroreduction of acetylene, the problems of low ethylene yield and ease of inactivation in traditional catalysts are solved, and efficient ethylene preparation and acetylene removal in ethylene-acetylene mixture are achieved, which significantly improves the catalyst Stability and preparation efficiency.

CN119061423APending Publication Date: 2024-12-03XI AN JIAOTONG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411494612.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional heterogeneous catalysts have problems such as low ethylene yield, many by-products, easy deactivation, complex structure and high preparation cost in acetylene electroreduction, which limits their wide application.

Method used

Using a dual-core copper molecular catalyst, the dual-core copper molecules containing 1,5-cyclooctadiene are mixed with dispersant and binder, and then loaded on the gas diffusion layer after ultrasonic dispersion, and electrolytic cell devices are built to perform acetylene electrical reduction, so as to achieve Efficient preparation of ethylene and removal of acetylene in ethylene-acetylene mixture.

Benefits of technology

It significantly improves ethylene yield, reduces by-product generation, ensures long-term stability of the catalyst, simplifies the preparation process, reduces production costs, and achieves efficient electroreduction and impurity removal of acetylene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061423A_ABST
    Figure CN119061423A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing ethylene through acetylene electroreduction by using a binuclear copper molecular catalyst and removing impurities from acetylene in ethylene-acetylene mixed gas, which comprises the following steps: mixing the binuclear copper molecular catalyst containing 1, 5-cyclooctadiene pair with a dispersant and a binder, and carrying out ultrasonic dispersion to obtain catalyst slurry; uniformly loading the catalyst slurry on the gas diffusion layer, and drying to obtain a gas diffusion electrode; a gas diffusion electrode is used as a cathode to build an electrolytic tank device, acetylene reduction is carried out, the copper-based molecular catalyst shows excellent catalytic performance under ampere-level current, acetylene impurity removal (acetylene is smaller than 5 ppm) in ethylene and ethylene-acetylene mixed gas prepared through efficient acetylene electroreduction is achieved, and the activity of the copper-based molecular catalyst is remarkably superior to that of a traditional heterogeneous catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalytic design, and in particular relates to a method for realizing acetylene electroreduction to prepare ethylene and acetylene impurity removal in ethylene-acetylene mixed gas using a binuclear copper molecule catalyst. Background Art

[0002] Acetylene electroreduction to produce ethylene and acetylene impurity removal in ethylene-acetylene mixed gas are important because ethylene is a key raw material in the chemical industry and is widely used in plastics, chemical fibers and other fields, and acetylene impurities in the mixed gas will affect the purity of ethylene and the quality of downstream products. Through efficient acetylene electroreduction and impurity removal methods, not only can the production efficiency and purity of ethylene be improved, but also the production cost and energy consumption can be reduced, promoting the development of green chemical industry.

[0003] There are many scientific and technological problems in the field of acetylene impurity removal in the electroreduction of acetylene to produce ethylene and ethylene-acetylene mixed gas by traditional heterogeneous catalysts. First, traditional catalysts usually have low selectivity and activity, resulting in low ethylene yield and many by-products. Secondly, these catalysts are easily deactivated at high current density and cannot operate stably for a long time. In addition, the structure of heterogeneous catalysts is complex, and the active sites are difficult to accurately control, resulting in poor controllability of the catalytic process. Finally, the preparation and recovery process of the catalyst is complicated and the cost is high, making it difficult to achieve large-scale application. These problems restrict the widespread application of traditional heterogeneous catalysts in the field of acetylene electroreduction and impurity removal. Summary of the invention

[0004] In order to overcome the problem of low ethylene yield in the conventional heterogeneous catalyst in the prior art when acetylene is electro-reduced, the object of the present invention is to provide a method for realizing acetylene electro-reduction to prepare ethylene and acetylene impurity removal in ethylene-acetylene mixed gas by using a binuclear copper molecule catalyst. The method can realize acetylene electro-reduction to prepare ethylene and acetylene impurity removal in ethylene-acetylene mixed gas under ampere-level current, and the ethylene yield is high.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A method for preparing ethylene by electroreduction of acetylene using a binuclear copper molecule catalyst and removing impurities from acetylene in an ethylene-acetylene mixed gas, comprising the following steps: The binuclear copper molecule catalyst containing 1,5-cyclooctadiene pairs is mixed with a dispersant and a binder and ultrasonically dispersed to obtain a catalyst slurry; The catalyst slurry is evenly loaded on the gas diffusion layer and dried to obtain a gas diffusion electrode; An electrolytic cell device is constructed using the gas diffusion electrode as the cathode to carry out acetylene reduction.

[0006] A further improvement of the present invention is that the binuclear copper molecule catalyst containing 1,5-cyclooctadiene is (1,5-cyclooctadiene) copper chloride dimer.

[0007] A further improvement of the present invention is that the dispersant is at least one of isopropanol, ethanol, acetone and water.

[0008] A further improvement of the present invention is that the binder is a 5% Nafion solution.

[0009] A further improvement of the present invention is that the usage ratio of the binuclear copper molecule catalyst, the dispersant and the binder is 3 mg: 600 µL: 4 µL.

[0010] A further improvement of the present invention is that the loading method is spraying or dipping.

[0011] A further improvement of the present invention is that the catalyst slurry has a loading mass of 0.1-10 mg·cm -3 .

[0012] A further improvement of the present invention is that the electrolytic cell device is a flow electrolytic cell device or a membrane electrode electrolytic cell.

[0013] A further improvement of the present invention is that when the electrolytic cell device is a flow electrolytic cell device, 1 mol / L potassium hydroxide is used as the cathode and anode electrolytes, an anion exchange membrane is used for isolation, Hg / HgO or Ag / AgCl is used as a reference electrode, nickel foam is used as a counter electrode, and a gas with an acetylene gas volume content of 1%-100% is used as a reaction gas, wherein the flow rate of the anode and cathode electrolytes is 1-100sccm, and the flow rate of the reaction gas is 1-100sccm.

[0014] A further improvement of the present invention is that when the electrolytic cell device is a membrane electrode electrolytic cell device, 1 mol / L potassium hydroxide is used as the cathode and anode electrolytes, an anion exchange membrane is used for isolation, nickel foam is used as the counter electrode, and 1%-100% acetylene gas is used as the reaction gas, wherein the flow rate of the anode and cathode electrolytes is 1-100sccm, and the flow rate of the reaction gas is 1-100sccm.

[0015] Compared with the prior art, the present invention has the following beneficial effects: Since 1,5-cyclooctadiene can form coordination compounds with transition metal ions with more d electrons in binuclear copper molecular catalysts, after forming dual coordination with copper, 1,5-cyclooctadiene can stabilize the metal center and adjust the electronic state of the metal, so that copper exhibits excellent acetylene semi-hydrogenation activity. The binuclear copper molecular catalyst of the present invention is active enough to surpass traditional metal catalysts in acetylene electroreduction; the molecular catalyst of the present invention can be directly used in heterogeneous electrocatalytic reactions, has excellent practical utilization value, and can achieve efficient acetylene electroreduction at ampere-level current; at the same time, in the experiment of removing acetylene impurities with ethylene-rich gas flow, acetylene impurities can be removed near the theoretical current, and almost no hydrogen is generated in the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a comparison diagram of polarization curves of the catalysts of Example 1, Example 2, and Example 3.

[0017] Figure 2 The catalysts of Example 1, Example 2 and Example 3 are -2 Comparison of Faraday efficiency distribution under current density.

[0018] Figure 3 This is the Faraday efficiency distribution diagram of (1,5-cyclooctadiene) copper chloride dimer in Example 1 using a flow electrolytic cell at different currents.

[0019] Figure 4 This is the Faraday efficiency distribution diagram of the (1,5-cyclooctadiene) copper chloride dimer in Example 4 at different currents using a two-electrode DC power supply.

[0020] Figure 5 This is a graph showing the data for removing impurities from a crude ethylene gas stream containing acetylene impurities using a membrane electrode as an electrolytic cell in Example 5 using (1,5-cyclooctadiene) copper chloride dimer.

[0021] Figure 6 The (1,5-cyclooctadiene) copper chloride dimer in Example 6 is 200 mA·cm -2 Long-term stability test diagram under current density. DETAILED DESCRIPTION

[0022] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.

[0023] Molecular catalysts have significant advantages and wide application potential in solving the problems faced by traditional heterogeneous catalysts. First, molecular catalysts have a clear molecular structure, so that the active site can be precisely regulated, thereby improving selectivity and activity, significantly improving ethylene yield and reducing the generation of by-products. Secondly, molecular catalysts can show excellent stability at high current density, can operate stably for a long time, and overcome the problem of easy deactivation of traditional catalysts. In addition, the synthesis process of molecular catalysts is relatively simple and highly repeatable, which is conducive to large-scale production and application. Finally, molecular catalysts have strong controllability in the catalytic process, can better adjust the reaction conditions, and improve reaction efficiency. Therefore, molecular catalysts are used in the present invention to carry out acetylene electroreduction.

[0024] The present invention provides a method for realizing acetylene electroreduction to prepare ethylene and acetylene impurity removal in ethylene-acetylene mixed gas by using a binuclear copper molecule catalyst, comprising the following steps: S1: mixing the molecular catalyst with the dispersant and the binder and performing ultrasonic dispersion to obtain a catalyst slurry; Wherein, the molecular catalyst includes but is not limited to (1,5-cyclooctadiene) copper chloride dimer.

[0025] The dispersant includes but is not limited to at least one of isopropanol, ethanol, acetone and water.

[0026] The binder includes but is not limited to 5% Nafion solution.

[0027] S2: The obtained catalyst slurry is uniformly loaded on a gas diffusion layer (commercial carbon paper), and after natural drying, a gas diffusion electrode is obtained; Wherein, the loading method includes but is not limited to spraying and dipping.

[0028] The catalyst slurry has a loading mass of 0.1-10 mg·cm on the gas diffusion layer. -3 .

[0029] S3: Using the obtained gas diffusion electrode as a cathode to construct an electrolytic cell device for acetylene reduction.

[0030] Wherein, the electrolytic cell device is a flow cell electrolytic cell device or a membrane electrode electrolytic cell.

[0031] When the electrolytic cell device is a flow cell device, 1 mol / L potassium hydroxide is used as the cathode and anode electrolyte, an anion exchange membrane is used for isolation, Hg / HgO or Ag / AgCl is used as the reference electrode, nickel foam is used as the counter electrode, and a gas containing 1%-100% acetylene volume concentration is used as the reaction gas. The flow rate of the cathode and anode electrolyte is 1-100 sccm, and the flow rate of the reaction gas is 1-100 sccm.

[0032] When the electrolytic cell device is a membrane electrode electrolytic cell device, 1 mol / L potassium hydroxide is used as the cathode and anode electrolyte, an anion exchange membrane is used for isolation, nickel foam is used as the counter electrode, and 1%-100% acetylene gas is used as the reaction gas. The flow rate of the cathode and anode electrolyte is 1-100 sccm, and the flow rate of the reaction gas is 1-100 sccm.

[0033] In the specific test, an electrochemical workstation and a DC power supply were used to test the electrochemical performance of electrocatalytic acetylene reduction. The electrochemical activity of the catalyst was tested by linear sweep voltammetry, and the reaction activity of the catalyst was tested by constant current mode. A gas chromatograph was used to detect the product content. The FID detector was used to detect C2H2, C2H4, C2H6, butadiene, and the TCD detector was used to detect H2.

[0034] Example 1 Disperse 3 mg of (1,5-cyclooctadiene) copper chloride dimer in 600 µL of isopropanol and 4 µL of 5% Nafion solution, and ultrasonicate for 30 minutes to obtain a catalyst slurry. Spray 200 µL of the obtained slurry onto a 1 cm 2 The gas diffusion electrode was loaded with 1 mg cm -2 A gas diffusion electrode was used as the battery cathode; nickel foam was used as the battery anode, Hg / HgO as the reference electrode, and 1 mol / L KOH solution as the anode electrolyte, which were separated by an anion exchange membrane to assemble a flow cell; a peristaltic pump was used to control the cathode electrolyte flow rate to 10 sccm, and the anode electrolyte was controlled in flushing mode; a gas mass flowmeter was used to control the reaction gas flow rate to 20 sccm, and high-purity acetylene was used as the reaction gas; an electrochemical workstation was used to test the electrochemical activity of the catalyst by linear sweep voltammetry, and a constant current mode was used to test the reaction activity of the catalyst, and a gas chromatograph was used to detect the product content and calculate the Faraday efficiency.

[0035] See also Figure 3 It can be seen that the Faraday efficiency of the catalyst in producing ethylene exceeds 90%, and it has excellent acetylene semi-hydrogenation activity.

[0036] Comparative Example 1 Disperse 3 mg (1,5-cyclooctadiene) rhodium chloride dimer in 600 µL isopropanol and 4 µL 5% Nafion solution, and ultrasonicate for 30 minutes to obtain catalyst slurry; spray 200 µL of the obtained slurry to 1 cm 2 The gas diffusion electrode was loaded with 1 mg cm -2A gas diffusion electrode was used as the battery cathode; nickel foam was used as the battery anode, Hg / HgO as the reference electrode, and 1 mol / L KOH solution as the anode electrolyte, which were separated by an anion exchange membrane to assemble a flow cell; a peristaltic pump was used to control the cathode electrolyte flow rate to 10 sccm, and the anode electrolyte was controlled in flushing mode; a gas mass flowmeter was used to control the reaction gas flow rate to 20 sccm, and high-purity acetylene was used as the reaction gas; an electrochemical workstation was used to test the electrochemical activity of the catalyst by linear sweep voltammetry, and a constant current mode was used to test the reaction activity of the catalyst, and a gas chromatograph was used to detect the product content and calculate the Faraday efficiency.

[0037] Comparative Example 2 Disperse 3 mg (1,5-cyclooctadiene) platinum dichloride in 600 µL isopropanol and 4 µL 5% Nafion solution, and ultrasonicate for 30 minutes to obtain a catalyst slurry. Spray 200 µL of the obtained slurry onto a 1 cm 2 The gas diffusion electrode was loaded with 1 mg cm -2 A gas diffusion electrode was used as the battery cathode; nickel foam was used as the battery anode, Hg / HgO as the reference electrode, and 1 mol / L KOH solution as the anode electrolyte, which were separated by an anion exchange membrane to assemble a flow cell; a peristaltic pump was used to control the cathode electrolyte flow rate to 10 sccm, and the anode electrolyte was controlled in flushing mode; a gas mass flowmeter was used to control the reaction gas flow rate to 20 sccm, and high-purity acetylene was used as the reaction gas; an electrochemical workstation was used to test the electrochemical activity of the catalyst by linear sweep voltammetry, and a constant current mode was used to test the reaction activity of the catalyst, and a gas chromatograph was used to detect the product content and calculate the Faraday efficiency.

[0038] See also Figure 1 and Figure 2 It can be seen that the current density of Example 1 at the same voltage is significantly greater than that of Comparative Example 2 and Comparative Example 3, and the Faraday efficiency of Example 1 for ethylene survival at the same current density is significantly greater than that of Comparative Example 2 and Comparative Example 3, and Example 1 has higher intrinsic activity for the reaction.

[0039] Example 2 Disperse 3 mg of (1,5-cyclooctadiene) copper chloride dimer in 600 µL of isopropanol and 4 µL of 5% Nafion solution, and ultrasonicate for 30 minutes to obtain a catalyst slurry. Spray 200 µL of the obtained slurry onto a 1 cm 2 The gas diffusion electrode was loaded with 1 mg cm -2A gas diffusion electrode was used as the battery cathode; nickel foam was used as the battery anode, and 1 mol / L KOH solution was used as the anode and cathode electrolytes, which were separated by an anion exchange membrane to assemble a two-electrode flow cell; a peristaltic pump was used to control the cathode electrolyte flow rate to 10 sccm, and the anode electrolyte was controlled in flushing mode; a gas mass flow meter was used to control the reaction gas flow rate to 20 sccm, and high-purity acetylene was used as the reaction gas; a DC power supply was used to test the reaction activity of the catalyst in a two-electrode constant current mode, and a gas chromatograph was used to detect the product content and calculate the Faraday efficiency.

[0040] See also Figure 4 It can be seen that the catalyst also maintains high activity when using DC power supply, at 800 mA·cm -2 The Faradaic efficiency of ethylene can be maintained at nearly 90% at low current density.

[0041] Example 3 Disperse 30 mg of (1,5-cyclooctadiene) copper chloride dimer in 6000 µL of isopropanol and 40 µL of 5% Nafion solution, and ultrasonicate for 30 minutes to obtain a catalyst slurry. Spray 5000 µL of the obtained slurry onto a 25 cm 2 The gas diffusion electrode was loaded with 1 mg cm -2 A gas diffusion electrode was used as the battery cathode; nickel foam was used as the battery anode, and 1 mol / L KOH solution was used as the anode and cathode electrolytes, which were separated by an anion exchange membrane to assemble a membrane electrode electrolytic cell; a peristaltic pump was used to control the cathode electrolyte flow rate to 10 sccm, and the anode electrolyte was controlled in flushing mode; a gas mass flowmeter was used to control the reaction gas flow rate to 20 sccm, and the reaction gas used was a crude ethylene mixture (volume percentage of 0.5% C2H2, 20% C2H4, Ar filling); an electrochemical workstation was used to test the catalyst's de-doping reaction activity in constant current mode, and a gas chromatograph was used to detect the product content.

[0042] See also Figure 5 It can be seen that this molecular catalyst has excellent impurity removal activity, has practical application prospects, and almost no hydrogen is generated.

[0043] Example 4 Disperse 3 mg of (1,5-cyclooctadiene) copper chloride dimer in 600 µL of isopropanol and 4 µL of 5% Nafion solution, and ultrasonicate for 30 minutes to obtain a catalyst slurry. Spray 200 µL of the obtained slurry onto a 1 cm 2 The gas diffusion electrode was loaded with 1 mg cm -2A gas diffusion electrode was used as the battery cathode; nickel foam was used as the battery anode, Hg / HgO as the reference electrode, and 1 mol / L KOH solution as the anode electrolyte, which were separated by an anion exchange membrane to assemble a flow cell; a peristaltic pump was used to control the cathode electrolyte flow rate to 10 sccm, and the anode electrolyte was controlled in flushing mode; a gas mass flow meter was used to control the reaction gas flow rate to 20 sccm, and high-purity acetylene was used as the reaction gas; an electrochemical workstation was used to control the reaction current to 200 mA in constant current mode, and the long-term stability of the catalyst was tested. A gas chromatograph was used to detect the product content and calculate the Faraday efficiency.

[0044] See also Figure 6 It can be seen that the voltage of the catalyst remained stable within 72 h and the activity did not decrease, showing good stability.

[0045] Example 5 Same as Example 1, except that the dispersant is ethanol and the loading mass of the catalyst slurry on the gas diffusion layer is 0.1 mg cm -3 .

[0046] Example 6 Same as Example 1, except that the dispersant is acetone and the loading mass of the catalyst slurry on the gas diffusion layer is 5 mg cm -3 .

[0047] Example 7 Same as Example 1, except that the dispersant is water and the loading mass of the catalyst slurry on the gas diffusion layer is 10 mg cm -3 .

[0048] The present invention uses 1,5-cyclooctadiene chloride as a molecular catalyst, uses a gas diffusion layer electrode loaded with the catalyst as a cathode, assembles a flow electrolysis cell or a membrane electrode electrolysis cell, and realizes efficient acetylene electroreduction to prepare ethylene and acetylene impurity removal in ethylene-acetylene mixed gas (acetylene is less than 5ppm). The copper-based molecular catalyst of the present invention exhibits excellent catalytic performance under ampere-level current, realizes efficient acetylene electroreduction to prepare ethylene and acetylene impurity removal in ethylene-acetylene mixed gas, and its activity is significantly better than that of traditional heterogeneous catalysts.

[0049] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.

[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

Claims

1. A method for preparing ethylene by electroreduction of acetylene using a binuclear copper molecule catalyst and removing acetylene impurities from ethylene-acetylene mixed gas, characterized in that: The following steps are involved: The binuclear copper molecule catalyst containing 1,5-cyclooctadiene pairs is mixed with a dispersant and a binder and ultrasonically dispersed to obtain a catalyst slurry; The catalyst slurry is evenly loaded on the gas diffusion layer and dried to obtain a gas diffusion electrode; An electrolytic cell device is constructed using the gas diffusion electrode as the cathode to carry out acetylene reduction.

2. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The binuclear copper molecule catalyst containing 1,5-cyclooctadiene is (1,5-cyclooctadiene) copper chloride dimer.

3. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The dispersant is at least one of isopropanol, ethanol, acetone and water.

4. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The binder is 5% Nafion solution.

5. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The dosage ratio of binuclear copper molecule catalyst, dispersant and binder is 3mg:600µL:4µL.

6. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The loading method is spraying or dipping.

7. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The catalyst slurry has a loading mass of 0.1-10 mg·cm on the gas diffusion layer. -3 .

8. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 1, characterized in that: The electrolytic cell device is a flow electrolytic cell device or a membrane electrode electrolytic cell.

9. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 8, characterized in that: When the electrolytic cell device is a flow electrolytic cell device, 1 mol / L potassium hydroxide is used as cathode and anode electrolyte, an anion exchange membrane is used for isolation, Hg / HgO or Ag / AgCl is used as a reference electrode, nickel foam is used as a counter electrode, and a gas with an acetylene gas volume content of 1%-100% is used as a reaction gas, wherein the flow rate of the cathode and anode electrolyte is 1-100sccm, and the flow rate of the reaction gas is 1-100sccm.

10. The method for preparing ethylene by electroreduction of acetylene and removing impurities from ethylene-acetylene mixed gas by using binuclear copper molecule catalyst according to claim 8, characterized in that: When the electrolytic cell device is a membrane electrode electrolytic cell device, 1 mol / L potassium hydroxide is used as the cathode and anode electrolyte, an anion exchange membrane is used for isolation, foam nickel is used as the counter electrode, and 1%-100% acetylene gas is used as the reaction gas, wherein the flow rate of the cathode and anode electrolyte is 1-100sccm, and the flow rate of the reaction gas is 1-100sccm.

Citation Information

Cited By

  • Method for carrying out electrocatalytic hydrogenation on alkynol by using copper acetylacetonate molecular catalyst