V2C / V2O5 / NiO composite gas-sensitive material as well as preparation method and application thereof
Through V2C/V2O5/NiO composite materials, the lack of sensitivity and high-temperature operation of nickel oxide and V2O5 in gas sensors are solved, and the rapid response and recovery of methane gas is achieved, with good selectivity and low-temperature detection capabilities, suitable for 500ppm ~4000ppm concentration range.
Patent Information
- Application Number
- CN202411449847.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-17
AI Technical Summary
The existing nickel oxide and V2O5 materials have problems such as insufficient sensitivity, slow response speed, poor low temperature detection capability and high temperature operation in gas sensors, which limit their application in complex environments.
V2C/V2O5/NiO composite gas-sensitive material is used to prepare V2C MXene through the reaction of HF, HCl, water and V2AlC, and combined with Ni-MOF material. After calcination, V2C/V2O5/NiO composite material is formed for methane gas In the sensor, the p-type semiconductor properties of NiO and the redox properties of V2O5 are used to improve the gas-sensitive performance.
It achieves rapid response and recovery to methane gas, has good selectivity and low temperature detection capabilities, and is suitable for concentration ranges of 500ppm to 4000ppm, reducing the slow response speed of traditional sensors and insufficient durability under high-temperature operating conditions.
Smart Images

Figure CN119064426A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of gas sensors, and in particular relates to a V2C / V2O5 / NiO composite gas-sensitive material and a preparation method and application thereof. Background Art
[0002] Methane gas (CH4) is a colorless, odorless gas. It is the simplest hydrocarbon compound and one of the most important greenhouse gases in nature. It is ubiquitous in industrial production, natural gas extraction, landfills and agriculture. Methane leakage not only causes waste of resources, but also leads to the intensification of the greenhouse effect, which has an important impact on global climate change. In addition, methane has a certain degree of explosiveness. If the concentration reaches a certain range, it will pose a threat to production safety and human life safety. Therefore, in order to effectively monitor and control the emission of methane gas and protect human health and the environment, it is urgent to develop cost-effective, highly sensitive and highly selective methane gas sensors. Such sensors will be able to detect the presence of methane in a timely and accurate manner, providing important technical support for leakage prevention, emission reduction and environmental monitoring.
[0003] Nickel oxide (NiO) is a metal oxide with obvious semiconductor properties, usually presenting a variety of crystal structures and having good chemical stability. In the field of gas sensors, nickel oxide is widely used to detect a variety of harmful gases. Due to its excellent conductivity and high surface activity, nickel oxide materials show good gas-sensing properties in the gas detection process. However, unmodified nickel oxide needs to be operated at a higher temperature to show good gas-sensing properties, and there are certain limitations in gas sensitivity. This is mainly because at high temperatures, the conductivity of nickel oxide increases, and the interaction between gas molecules and the material surface becomes more significant, thereby improving the sensitivity of the sensor. The low surface activity of nickel oxide leads to a decrease in the reaction rate between the gas and the sensor surface, thereby affecting the response time and sensitivity of the sensor. The surface reactivity of pure nickel oxide is not strong enough, which limits its effective chemical reaction with gas molecules. In the gas detection process, nickel oxide with low surface activity cannot provide sufficient gas-solid interface reaction, thereby affecting the sensitivity of gas detection. However, high-temperature operation poses a challenge to the long-term stability and reliability of the sensor, and may lead to increased energy consumption and material aging. This phenomenon makes it more difficult to detect specific gases in complex environments. Therefore, in order to improve the performance and application effect of nickel oxide in gas sensors, it is urgent to modify it to enhance the sensitivity and reduce the operating temperature, thereby achieving more efficient gas detection.
[0004] V2C is a new type of transition metal carbide with excellent electronic conductivity and mechanical strength, and its derivative oxide V2O5 shows broad application prospects. V2O5 has become an important material in the field of catalysis and energy storage due to its excellent electrocatalytic activity, good chemical stability and high specific surface area. V2O5 has also attracted widespread attention in the field of gas sensors, mainly due to its excellent redox properties and electron transfer ability. In particular, the multivalent oxide characteristics of V2O5 enable it to react with a variety of gases and show good gas sensitivity. However, pure V2O5 materials often face problems of large resistance and high operating temperature requirements in practical applications. These limiting factors may affect its performance and applicability in actual gas sensors. Therefore, it is an important direction of current research to optimize the performance of V2O5 and improve its low-temperature operation to enhance its application effect in gas sensors. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a V2C / V2O5 / NiO composite gas-sensitive material and a preparation method and application thereof.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] One of the technical solutions of the present invention is to provide a method for preparing a V2C / V2O5 / NiO composite gas-sensitive material, comprising the following steps:
[0008] HF, HCl, water and V2AlC are mixed and reacted, and the product is washed with water until the pH value is 6 to 7 to obtain V2C MXene material;
[0009] Dissolving dimethylimidazole, nickel nitrate and benzenetricarboxylic acid in a solvent, stirring them evenly and then performing a solvothermal reaction to prepare a Ni-MOF material;
[0010] The V2C MXene material and the Ni-MOF material are co-dispersed in a solvent and then the solvent is removed to obtain a preliminary composite material, and the preliminary composite material is calcined to obtain a V2C / V2O5 / NiO composite gas-sensitive material.
[0011] Preferably, the usage ratio of HF, HCl, water and V2AlC is 10 mL:10 mL:5 mL:1 g; the temperature of the mixed reaction is 40° C. and the time is 48 h.
[0012] Preferably, the molar ratio of dimethylimidazole, nickel nitrate and trimesic acid is 1:1:1; the temperature of the solvent thermal reaction is 180° C. and the time is 48 hours.
[0013] Preferably, the preliminary composite material is obtained by compounding a V2C MXene material and a Ni-MOF material in a mass ratio of 1:2.
[0014] Preferably, the calcination temperature is 600-700° C., the holding time is 2-3 hours, and the heating rate is 1-3° C. / min.
[0015] The second technical solution of the present invention: provides a V2C / V2O5 / NiO composite gas-sensitive material prepared according to the preparation method of the above-mentioned V2C / V2O5 / NiO composite gas-sensitive material.
[0016] The third technical solution of the present invention: provides an application of the above-mentioned V2C / V2O5 / NiO composite gas-sensitive material in the preparation of a methane gas sensor, wherein the gas-sensitive coating of the gas-sensitive element of the methane gas sensor is a V2C / V2O5 / NiO composite gas-sensitive material.
[0017] The sensing mechanism of the methane gas sensor provided by the present invention is:
[0018] First, NiO exhibits p-type semiconductor properties, and the main carriers are holes. When NiO is exposed to air, oxygen molecules adsorb on the NiO surface and capture electrons to form chemically adsorbed oxygen, resulting in the formation of a hole accumulation layer on the NiO surface. Secondly, when NiO is exposed to methane gas, methane gas molecules adsorb on the surface of the sensitive material, react with the surface chemically adsorbed oxygen, and then release electrons back to the semiconductor, resulting in a decrease in the thickness of the hole accumulation layer, and ultimately an increase in the sensor resistance. In addition, since the work function of V2O5 is smaller than that of NiO, electrons flow from V2O5 to NiO, forming a pn heterojunction between V2O5 and NiO. A space charge region is formed at the junction, and a hole depletion layer is formed on the NiO surface, resulting in a larger baseline resistance of the V2O5 / NiO composite material. When the V2C / V2O5 / NiO sensor is exposed to methane, the methane gas reacts with the adsorbed oxygen, and the trapped electrons return to the semiconductor to neutralize some holes, thereby widening the hole depletion layer and increasing the barrier height of the hole depletion layer, resulting in a significant increase in resistance. In addition, since the multilayer V2C MXene derives a "noodle"-like V2C / V2O5 nanoporous structure, it is conducive to the adsorption and diffusion of CH4 gas molecules. After NiO nanoparticles are attached to the surface of V2C / V2O5, the surface reaction sites of the material are greatly increased, which is conducive to the surface reaction, thereby improving the gas-sensing performance of the composite material.
[0019] The beneficial technical effects of the present invention are as follows:
[0020] The present invention partially oxidizes V2C MXene, derives V2O5 nanoblocks on the V2C MXene layered structure, obtains uniformly distributed "instant noodles" structure nano V2O5, obtains NiO nanoparticles by heat treating Ni-MOF, and synthesizes a V2C / V2O5 / NiO composite gas-sensitive structure. The methane sensor prepared from the V2C / V2O5 / NiO composite film has the advantages of reversible model, fast response / recovery speed, good selectivity, etc. The concentration detection range of methane gas is 500ppm~4000ppm, and even low concentration of methane gas can be effectively detected, and the detection temperature is low, which effectively solves the shortcomings of traditional methane gas sensors such as slow response speed, poor sensitivity at low concentration, and poor durability under high temperature working conditions, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a flow chart for preparing the V2C / V2O5 / NiO composite gas-sensitive material in Example 1 of the present invention.
[0022] Figure 2 This is a schematic diagram of the structure of the methane gas sensor in Example 1 of the present invention, wherein 1 is a substrate, 2 is an interdigitated electrode substrate, 3 is a Cr / Ni / Au alloy interdigitated electrode, and 4 is a gas-sensitive coating.
[0023] Figure 3 This is the SEM image of the V2C / V2O5 / NiO composite gas-sensitive material prepared in Example 1, where (a) and (b) are SEM images at different magnifications.
[0024] Figure 4 This is the X-ray diffraction pattern of the V2C / V2O5 / NiO composite gas-sensitive material prepared in Example 1.
[0025] Figure 5 This is a resistance diagram of the methane gas sensor prepared in Example 1 responding to 500ppm-4000ppm methane gas at an operating temperature of 200°C.
[0026] Figure 6 It is a fitting curve diagram of the response of the methane gas sensor prepared in Example 1 and the comparative methane gas sensor to methane gas of various concentrations at an operating temperature of 200°C.
[0027] Figure 7 The sensitivity curves of the methane gas sensor prepared in Example 1 and the comparative methane gas sensor to 4000 ppm methane gas at different operating temperatures are shown.
[0028] Figure 8This is a repeatability test graph of the response resistance of the methane gas sensor prepared in Example 1 to 2000ppm and 4000ppm methane gas at an operating temperature of 200°C.
[0029] Fig. 9 This is a test diagram of the response / recovery characteristics of the methane gas sensor prepared in Example 1 to 2000 ppm methane gas at an operating temperature of 200°C.
[0030] Fig.10 This is a graph showing the selectivity of the methane gas sensor prepared in Example 1 to different types of gases at an operating temperature of 200°C. DETAILED DESCRIPTION
[0031] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0032] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0033] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0035] Example 1
[0036] Preparation of multilayer V2C MXene: Add 20 mL HF, 20 mL HCl and 10 mL deionized water to 250 mL polytetrafluoroethylene liner to obtain a mixed solution, add 2 g V2AlC to the mixed solution, and react with magnetic stirring at 40 degrees for 48 hours. Then, wash the black precipitate repeatedly with deionized water until the pH value is between 6 and 7, and then dry it in a vacuum oven at 80°C for 8 hours.
[0037] Preparation of Ni-MOF powder: 2mmol dimethylimidazole, 2mmol Ni(NO3)2·6H2O and 2mmol benzenetricarboxylic acid were dissolved in 100mL dimethylformamide solution and stirred continuously at room temperature for 1h. After that, the solution was transferred to a 100mL polytetrafluoroethylene liner, reacted at 180℃ for 48h and cooled to room temperature. Ni-MOF was washed with anhydrous ethanol by centrifugation 3 times and then dried in a vacuum oven at 80℃ for 8h.
[0038] The V2C MXene dispersion was mixed with the Ni-MOF dispersion, the mass ratio of V2C MXene to Ni-MOF was 1:2, the mixed dispersion was stirred continuously at room temperature for 1 hour, and then dried in a vacuum oven at 80°C. The resulting powder was then placed in a tube furnace, heated to 600°C at a heating rate of 2°C / min and kept warm for 2 hours. The resulting powder was the V2C / V2O5 / NiO composite gas-sensitive material. The preparation flow chart of the V2C / V2O5 / NiO composite gas-sensitive material is shown in Figure 1 .
[0039] Preparation of gas-sensitive elements: The V2C / V2O5 / NiO composite gas-sensitive material was ultrasonically treated for 0.5 h to fully dissolve it in deionized water to form a uniform paste, which was then applied to the Cr / Ni / Au interdigital electrode to form a gas-sensitive coating with a thickness of approximately 200 μm. The gas-sensitive element coated with the gas-sensitive coating was dried at 50°C for 5 h and aged at 300°C on an aging bench for 24 h.
[0040] Methane gas sensor: See the structural diagram Figure 2 It consists of an alumina ceramic heating substrate 1 at the bottom, a ceramic interdigital electrode substrate 2, a Cr / Ni / Au alloy interdigital electrode 3 and a gas sensitive coating 4 coated on the interdigital electrode 3.
[0041] The SEM image of the V2C / V2O5 / NiO composite gas-sensitive material prepared in Example 1 is shown in Figure 3 , where (a) and (b) are SEM images at different magnifications.
[0042] Depend on Figure 3 It can be seen that NiO nanoparticles are evenly distributed, the "instant noodles" structure nanoporous V2O5 is composed of blocky V2O5, and the surface is very rough with obvious cracks, which greatly increases the specific surface area of nano V2O5, and NiO nanoparticles and porous V2O5 have good connection in the V2C / V2O5 / NiO composite gas-sensitive material.
[0043] In the V2C / V2O5 / NiO composite gas-sensitive material prepared in Example 1, the diameter of NiO nanoparticles is 10-30 nm, and the length of V2O5 nanoblocks is 100-300 nm, the width is 100-200 nm, and the thickness is 50-100 nm.
[0044] The X-ray diffraction pattern of the V2C / V2O5 / NiO composite gas-sensitive material prepared in Example 1 is shown in Figure 4 .
[0045] Figure 4 All diffraction peaks belonging to V2C MXene, V2O5 and NiO are displayed, and there is no obvious diffraction of other crystalline phases, indicating that the purity of the prepared samples is very high.
[0046] The test method of sensor performance is: using air as carrier gas, different methane gas concentrations are prepared in the test box through standard methane sample gas. The sensor is switched between air and methane gas environments to test the sensor's repeatability, response / recovery, selectivity and other gas-sensitive performance. The switching time interval of the sensor is 180s (the same applies to other gases).
[0047] The response resistance diagram of the methane gas sensor prepared in Example 1 to 500ppm-4000ppm methane gas at an operating temperature of 200°C is shown in FIG. Figure 5 .
[0048] Depend on Figure 5 It can be seen that the methane gas sensor prepared in Example 1 has a faster response and recovery time. In 8 consecutive reaction cycles, it has good response reversibility to 500ppm~4000ppm of methane gas, and the resistance change shows an increasing trend with the increase of methane gas concentration.
[0049] The fitting curves of the responses of the methane gas sensor prepared in Example 1 and the comparative methane gas sensor to methane gas of various concentrations at an operating temperature of 200°C are shown in FIG. Figure 6 .
[0050] Figure 6 It shows that the sensitivity of V2C / V2O5 / NiO composite gas-sensitive material to 500ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm and 4000ppm methane gas is 9.5%, 16.4%, 25.9%, 30.5%, 37.1%, 41.9%, 47.3% and 56.8% respectively, with good linearity. The influence of V2C / V2O5 composite gas-sensitive material and NiO gas-sensitive material is significantly lower than that of V2C / V2O5 / NiO composite gas-sensitive material.
[0051] The sensitivity curves of the methane gas sensor prepared in Example 1 and the comparative methane gas sensor to 4000ppm methane gas at different working temperatures are shown in FIG. Figure 7 .
[0052] Depend on Figure 7 It can be seen that the optimal working temperature of V2C / V2O5 / NiO composite gas-sensitive material is 200℃.
[0053] The comparative methane gas sensor is a V2C / V2O5 composite gas-sensitive material and a NiO gas-sensitive material obtained by calcining the multilayer V2C MXene and Ni-MOF powder in Example 1 (the calcination conditions are the same as in Example 1), and a methane gas sensor is prepared by referring to the preparation method of the gas sensitive element and the methane gas sensor in Example 1 (the amount of gas sensitive material coated on the gas sensitive element is the same as in Example 1).
[0054] The repeatability test graph of the response resistance of the methane gas sensor prepared in Example 1 to 2000ppm and 4000ppm methane gas at an operating temperature of 200°C is shown in FIG. Figure 8 .
[0055] Depend on Figure 8 It can be seen that the methane gas sensor prepared in Example 1 has no obvious change in repeatability measurement for three reversible response cycles of 2000 and 4000 ppm methane gas, indicating that the sensor has good stability and repeatability.
[0056] The response / recovery characteristics test graph of the methane gas sensor prepared in Example 1 to 2000ppm methane gas at an operating temperature of 200°C is shown in FIG. Fig. 9 .
[0057] Depend on Fig. 9 It can be seen that the response and recovery time of the methane gas sensor prepared in Example 1 to 2000ppm methane gas are 72s and 113s respectively. The response time and recovery time are defined as the time it takes for the sensor to reach 90% of its final response value in the adsorption and desorption of the detection gas.
[0058] The selectivity of the methane gas sensor prepared in Example 1 to different types of gases at a working temperature of 200°C is shown in FIG. Fig.10 .
[0059] Depend on Fig.10 It can be seen that the sensitivity of the methane gas sensor prepared in Example 1 to the five detected gases is in the order of methane>ethane>hydrogen>sulfur dioxide>carbon monoxide, indicating that under the same detection conditions, the selectivity to methane gas is the best, while the selectivity to carbon monoxide gas is the worst.
[0060] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a V2C / V2O5 / NiO composite gas-sensitive material, characterized in that: The following steps are involved: HF, HCl, water and V2AlC are mixed and reacted, and the product is washed with water until the pH value is 6-7 to obtain V2C MXene material; Dimethylimidazole, nickel nitrate and benzenetricarboxylic acid are dissolved in a solvent, stirred evenly and then subjected to solvothermal reaction to prepare Ni-MOF material; The V2C MXene material and the Ni-MOF material are co-dispersed in a solvent and then the solvent is removed to obtain a preliminary composite material. The preliminary composite material is calcined to prepare a V2C / V2O5 / NiO composite gas-sensitive material.
2. The method for preparing the V2C / V2O5 / NiO composite gas-sensitive material according to claim 1, characterized in that: The usage ratio of HF, HCl, water and V2AlC is 10 mL:10 mL:5 mL:1 g; the temperature of the mixed reaction is 40° C. and the time is 48 h.
3. The method for preparing the V2C / V2O5 / NiO composite gas-sensitive material according to claim 1, characterized in that: The molar ratio of dimethylimidazole, nickel nitrate and benzenetricarboxylic acid is 1:1:1; the temperature of the solvent thermal reaction is 180° C. and the time is 48 hours.
4. The method for preparing the V2C / V2O5 / NiO composite gas-sensitive material according to claim 1, characterized in that: The preliminary composite material is obtained by compounding V2C MXene material and Ni-MOF material in a mass ratio of 1:
2.
5. The method for preparing the V2C / V2O5 / NiO composite gas-sensitive material according to claim 1, characterized in that: The calcination temperature is 600-700° C., the heat preservation time is 2-3 hours, and the heating rate is 1-3° C. / min.
6. A V2C / V2O5 / NiO composite gas-sensitive material prepared according to the method for preparing a V2C / V2O5 / NiO composite gas-sensitive material according to any one of claims 1 to 5.
7. Use of the V2C / V2O5 / NiO composite gas-sensitive material according to claim 6 in the preparation of a methane gas sensor, characterized in that: The gas-sensitive coating of the gas-sensitive element of the methane gas sensor is a V2C / V2O5 / NiO composite gas-sensitive material.
Citation Information
Patent Citations
Heterogeneous interface material based on oxygen plasma, preparation method and application
CN115763736A
ZnO / SiC nano heterojunction high-temperature ethanol gas sensor and preparation method thereof
CN116593537A
Cited By
EMC gas component prediction method based on V2C / V2O5 / SnO2 sensor and GRU-Attention
CN121633196A
An EMC gas component prediction method based on a V2C / V2O5 / SnO2 sensor and a GRU-Attention