Building protection coating and preparation method thereof
By introducing sodium sulfonate-based and phosphoramide structures into the aqueous acrylic resin coating for building protection, and using mesoporous titanium dioxide anti-aging agent with hydrated alumina-encapsulated aluminum oxide to form a dense crosslinking network, the coating is solved in high light and high humidity The problems of insufficient combustibility, waterproofness and aging resistance in the environment achieve better flame retardant, waterproofing and aging resistance.
Patent Information
- Application Number
- CN202411186573.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Water-based acrylic resin coatings for building protection have problems such as insufficient combustibility, waterproofness and aging resistance in high-light and high humidity environments, and it is difficult to meet the strict usage requirements.
The combination of acrylate copolymers, film forming additives, pigments, fillers, wetting agents, dispersants, thickeners, defoamers, leveling agents and anti-aging agents is generated through specific stirring steps and reaction processes. Mesoporous titanium dioxide anti-aging agent containing sodium sulfonate groups, phosphoramide structures and hydrated alumina envelopes form a dense crosslinking network and protective layer, improving the flame retardant, waterproof and aging resistance of the paint.
It significantly improves the flame retardant and smoke resistance, waterproofness and aging resistance of the paint, extends its service life, overcomes the high toxicity and large smoke problems of halogen flame retardants, and forms excellent building protection effects.
Smart Images

Figure BDA0005013687930000141 
Figure BDA0005013687930000151
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to a coating for building protection and a preparation method thereof. Background Art
[0002] With the progress and development of science and technology, people's living standards have gradually improved, and higher performance requirements have been put forward for building protective coatings. According to the different dispersion media, coatings can be divided into water-based coatings and solvent-based coatings. Compared with solvent-based coatings, water-based coatings have the characteristics of green, healthy, and environmentally friendly, and have become the trend and direction of the development of the coating industry. Water-based acrylic resin coatings have the advantages of excellent paint film properties, pollution resistance, acid and alkali resistance, and no damage to the appearance of the covered objects, and are widely used in the construction field. However, the flammability of acrylic coatings is still a problem that needs to be solved in actual use. Building protective coatings that are in harsh environments such as high light and high humidity for a long time require better aging resistance and waterproofness to maintain excellent performance in harsh environments and extend service life. Therefore, it is urgent to develop a suitable modification method to improve the flame retardancy, waterproofness and aging resistance of water-based acrylic resin coatings for building protection to meet increasingly stringent use requirements. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a building protective coating and a preparation method thereof.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A coating for building protection, comprising the following raw materials in parts by weight: 40-60 parts of acrylic copolymer, 5-7 parts of film-forming aid, 15-20 parts of pigment, 10-15 parts of filler, 0.3-0.5 parts of wetting agent, 0.4-0.8 parts of dispersant, 0.8-1.0 parts of thickener, 0.2-0.6 parts of defoamer, 0.3-0.5 parts of leveling agent, 1.0-1.5 parts of antioxidant and 30-40 parts of water;
[0006] The film-forming aid is propylene glycol methyl ether acetate, the pigment is titanium dioxide, the filler is hollow glass microspheres, the wetting agent is fatty alcohol polyoxyethylene ether (supplier: Xingtai Xinlan Technology Co., Ltd.), the dispersant is polyacrylic acid sodium salt dispersant, the thickener is hydroxyethyl cellulose, the defoamer is emulsified silicone oil (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd.), and the leveling agent is polyether-modified polysiloxane;
[0007] The preparation of the building protective coating comprises the following steps:
[0008] Step S1: Deionized water, defoamer, dispersant and wetting agent are placed in a dispersion tank, stirred at a speed of 500-600 r / min for 10-15 min, and then pigment and filler are added, and stirred at a speed of 1200-1300 r / min for 20-25 min to obtain a mixed system;
[0009] Step S2: adjusting the rotation speed to 500-600 r / min, adding an acrylic copolymer, a film-forming aid, a thickener, a defoamer, a leveling agent, and an antioxidant to the obtained mixed system, and stirring for 10-15 minutes to obtain a building protective coating;
[0010] Furthermore, the weight ratio of the defoaming agent added in step S1 and step S2 is 1:1, and the sum of the weights of the defoaming agent added in step S1 and step S2 is the total amount of the defoaming agent;
[0011] The preparation of the acrylic acid ester copolymer comprises the following steps:
[0012] Step A1: Add dimethylphosphoryl chloride to toluene, then add sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate, stir at 0-5°C for 2 hours, then heat to 40-50°C, reflux at constant temperature and stir for 1 hour, filter, extract and dry to obtain reaction product 1;
[0013] Further, the usage ratio of dimethylphosphoryl chloride, toluene, and sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate is 0.1 mol: 100-110 mL: 0.1 mol;
[0014] During the reaction of step A1, phosphorus oxychloride in dimethylphosphoryl chloride reacts with the amino group of sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate to generate a reaction product 1 containing phosphoramide;
[0015] Step A2: Add the reaction product 1 and ethyl acetate into a three-necked flask, heat to 45-55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1-1.5h to obtain the reaction product 2;
[0016] Further, the usage ratio of the reaction product 1, ethyl acetate, and sodium dithionite is 0.1 mol: 120-130 mL: 0.1-0.15 mol;
[0017] During the reaction of step A2, the nitro group of the reaction product 1 is reduced to an amino group to obtain the reaction product 2;
[0018] Step A3: Add the reaction product 2, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, and stir the mixture at a constant temperature for 10 hours to obtain a reaction product c;
[0019] Further, the dosage ratio of the reaction product 2, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01 5 mol: 125-135 mL; the dosage ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 25-35 mL; the dosage ratio of the mixed solution a and the mixed solution b is 130-140 mL: 30-40 mL;
[0020] During the reaction of step A3, the amino group of the reaction product 2 reacts with methacryloyl chloride to generate a reaction product c containing a terminal double bond;
[0021] Step A4: Add glycidyl methacrylate and reaction product c into a three-necked flask, start stirring, slowly heat up to 58-62° C., slowly add potassium persulfate solution into the flask within 20 min, stir and react at constant temperature for 4-5 h, then heat up to 64-66° C., continue stirring and reacting for 30 min, and cool to room temperature to obtain an acrylic acid ester copolymer;
[0022] Further, the dosage ratio of glycidyl methacrylate, reaction product c, and potassium persulfate solution is 0.17 mol: 0.20 mol: 35-40 mL, and the concentration of potassium persulfate solution is 0.014 g / mL;
[0023] During the reaction of step A4, under the action of potassium persulfate, glycidyl methacrylate and the reaction product c undergo free radical copolymerization to generate an acrylic copolymer;
[0024] The preparation of the antioxidant comprises the following steps:
[0025] Step B1: Add 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under normal pressure with stirring for 48 hours to obtain reaction product a;
[0026] Further, the usage ratio of 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 70-80 mL: 0.01 mol: 0.01-0.015 mol;
[0027] During the reaction of step B1, the cyano group of 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile is reduced to an amino group to obtain a reaction product a;
[0028] Step B2: Add the reaction product a, 4-bromo-3-nitrophenyl thiocyanate (supplier: Nanjing Shizhou Biotechnology Co., Ltd.) and methanol into a flask, add 2-dicyclohexylphosphino-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and stir at 80° C. under nitrogen protection for 4-5 hours, and vacuum dry at 50° C. to obtain the reaction product b;
[0029] Further, the amount ratio of the reaction product a, 4-bromo-3-nitrophenyl thiocyanate, methanol, 2-dicyclohexylphosphino-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.12 mol: 90-100 mL: 0.0020 g: 0.0020 g: 0.20-0.25 mol;
[0030] During the reaction of step B2, the amino group of the reaction product a undergoes a dehydrobromination coupling reaction with 4-bromo-3-nitrophenylthiocyanate to generate a reaction product b;
[0031] Step B3: Add the reaction product b to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under stirring at normal pressure for 48 hours to obtain the reaction product c;
[0032] Further, the amount ratio of the reaction product b, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 110-120 mL: 0.04 mol: 0.040-0.045 mol;
[0033] During the reaction of step B3, the cyano group and the nitro group of the reaction product b are reduced to amino groups to obtain the reaction product c;
[0034] Step B4: adding mesoporous titanium dioxide and reaction product c to ethanol, and then stirring under vacuum conditions for 6-8 hours, after the reaction is completed, centrifuging and drying to obtain the loaded product; adding the loaded product to deionized water, stirring for 10-20 minutes, adding sodium hexametaphosphate, continuing to stir and adjusting the pH of the system to alkaline, and then vigorously stirring and heating to 80°C, adjusting the pH of the system to 5-6, and then slowly adding sodium aluminate solution, stirring for 30-40 minutes, adjusting the pH to 7.0, filtering, washing with water, and drying to obtain an antioxidant;
[0035] Furthermore, the dosage ratio of mesoporous titanium dioxide, reaction product c, and ethanol is 0.5-1g: 3-5g: 60mL, and the volume fraction of ethanol is 95%; the dosage ratio of the loaded product, sodium hexametaphosphate, and sodium aluminate solution is 18-20g: 50-60mL: 15-20mL, and the concentration of the sodium aluminate solution is 0.1g / mL;
[0036] During the reaction of step B4, mesoporous titanium dioxide has a special mesoporous structure, and the small molecule reaction product c is loaded in the mesoporous titanium dioxide to obtain a loaded product; then sodium hexametaphosphate is used as a dispersant, and hydrated aluminum oxide forms a film on the surface of the mesoporous titanium dioxide to obtain an antioxidant.
[0037] Beneficial effects of the invention: The invention discloses a coating for building protection and a preparation method thereof, comprising the following raw materials: an acrylic copolymer, a film-forming aid, a pigment, a filler, a wetting agent, a dispersant, a thickener, a defoamer, a leveling agent, an antioxidant and water. The synthesized acrylic copolymer comprises a sodium sulfonate group, a phosphoramide structure, an epoxy group and the like in the molecule. The epoxy group can cross-link with the active amino group contained in the antioxidant, making the cross-linking network of the matrix denser and improving the water resistance of the coating; the sulfur element in the sodium sulfonate group generates non-combustible gases such as sulfur dioxide during combustion, diluting the concentration of combustible gases, and solidifies in the carbon layer in the form of sodium sulfate and sodium sulfite compounds, forming a dense and thick protective carbon layer, reducing heat transfer in the combustion area, and effectively preventing further combustion of the matrix, while inhibiting the release of smoke; the phosphoramide structure has a synergistic flame retardant effect produced by phosphorus and nitrogen flame retardants forming a dense carbon layer in the solid phase and generating nitrogen-containing non-combustible gases in the gas phase. In the solid phase, the phosphoramide structure and the sodium sulfonate group make the generated carbon layer denser and also produce a synergistic flame retardant effect; compared with halogen flame retardants, the phosphoramide structure and the sodium sulfonate group overcome the problems of high toxicity and large smoke after combustion during the flame retardant process, and can effectively improve the flame retardant and smoke suppression properties of the coating.
[0038] The synthesized antioxidant is obtained by loading small molecule reaction product c on mesoporous titanium dioxide, and then coating hydrated alumina on the surface of mesoporous titanium dioxide. The reaction product c contains active amino groups, thioether groups and hindered phenol structures. Mesoporous titanium dioxide has strong ultraviolet shielding performance. After coating the inert hydrated alumina on its surface, the photocatalytic activity of mesoporous titanium dioxide is inhibited, the matrix is inhibited from being photocatalytically degraded by nano-titanium dioxide, and the coating is prevented from yellowing, powdering or even falling off, so that the mesoporous titanium dioxide can better play the function of shielding ultraviolet rays; the active amino groups contained in the reaction product c can cross-link with the epoxy groups contained in the acrylic copolymer, making the cross-linked network of the matrix more compact and synergistically improving the waterproofness of the coating; the hindered phenol structure can capture the free radicals generated by the thermal oxidative aging reaction of the polymer, generate hydroperoxides and relatively stable phenol oxygen free radicals, thereby terminating the thermal oxidative aging reaction of the polymer molecules and inhibiting chain growth; and the thioether group can reduce and decompose the hydroperoxide. The synergistic effect of mesoporous titanium dioxide, hindered phenol structure and thioether group makes the coating have excellent aging resistance. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] An acrylic acid ester copolymer, the preparation of which comprises the following steps:
[0042] Step A1: Add dimethylphosphoryl chloride to toluene, then add sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate, stir at 0°C for 2 hours, then heat to 40°C, reflux and react at constant temperature for 1 hour, filter, extract and dry to obtain reaction product 1; the dosage ratio of dimethylphosphoryl chloride, toluene and sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate is 0.1 mol: 100 mL: 0.1 mol;
[0043] Step A2: Add the reaction product 1 and ethyl acetate into a three-necked flask, heat to 45°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1 hour to obtain the reaction product 2; the amount ratio of the reaction product 1, ethyl acetate and sodium dithionite is 0.1 mol: 120 mL: 0.1 mol;
[0044] Step A3: Add the reaction product 2, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add methacryloyl chloride to dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, and stir the mixture at a constant temperature for 10 hours to obtain a reaction product c; the amount ratio of the reaction product 2, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01 5 mol: 125 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 25 mL; the amount ratio of the mixed solution a to the mixed solution b is 130 mL: 30 mL;
[0045] Step A4: Add glycidyl methacrylate and reaction product c into a three-necked flask, start stirring, slowly heat up to 58° C., slowly add potassium persulfate solution into the flask within 20 min, stir and react at constant temperature for 4 h, then heat up to 64° C., continue stirring and react for 30 min, and cool to room temperature to obtain an acrylic acid ester copolymer; the dosage ratio of glycidyl methacrylate, reaction product c, and potassium persulfate solution is 0.17 mol: 0.20 mol: 35 mL, and the concentration of potassium persulfate solution is 0.014 g / mL.
[0046] Example 2
[0047] An acrylic acid ester copolymer, the preparation of which comprises the following steps:
[0048] Step A1: Add dimethylphosphoryl chloride to toluene, then add sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate, stir at 0°C for 2 hours, then heat to 45°C, reflux and react at constant temperature for 1 hour, filter, extract and dry to obtain reaction product 1; the dosage ratio of dimethylphosphoryl chloride, toluene and sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate is 0.1 mol: 105 mL: 0.1 mol;
[0049] Step A2: Add the reaction product 1 and ethyl acetate into a three-necked flask, heat to 50°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1.3h to obtain the reaction product 2; the amount ratio of the reaction product 1, ethyl acetate and sodium dithionite is 0.1mol:125mL:0.13mol;
[0050] Step A3: Add the reaction product 2, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add methacryloyl chloride to dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, and stir the mixture at a constant temperature for 10 hours to obtain a reaction product c; the amount ratio of the reaction product 2, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01 5 mol: 130 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 30 mL; the amount ratio of the mixed solution a to the mixed solution b is 135 mL: 35 mL;
[0051] Step A4: Add glycidyl methacrylate and reaction product c into a three-necked flask, start stirring, slowly heat up to 60° C., slowly add potassium persulfate solution into the flask within 20 min, stir and react at constant temperature for 4.5 h, then heat up to 65° C., continue stirring and react for 30 min, and cool to room temperature to obtain an acrylic acid ester copolymer; the dosage ratio of glycidyl methacrylate, reaction product c, and potassium persulfate solution is 0.17 mol: 0.20 mol: 37 mL, and the concentration of potassium persulfate solution is 0.014 g / mL.
[0052] Example 3
[0053] An acrylic acid ester copolymer, the preparation of which comprises the following steps:
[0054] Step A1: Add dimethylphosphoryl chloride to toluene, then add sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate, stir at 5°C for 2 hours, then heat to 50°C, reflux and react at constant temperature for 1 hour, filter, extract and dry to obtain reaction product 1; the dosage ratio of dimethylphosphoryl chloride, toluene and sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate is 0.1 mol: 110 mL: 0.1 mol;
[0055] Step A2: Add the reaction product 1 and ethyl acetate into a three-necked flask, heat to 55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1.5 hours to obtain the reaction product 2; the amount ratio of the reaction product 1, ethyl acetate and sodium dithionite is 0.1 mol: 130 mL: 0.15 mol;
[0056] Step A3: Add the reaction product 2, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add methacryloyl chloride to dimethyl sulfoxide to obtain a mixed solution b, slowly drop the mixed solution b into the mixed solution a under a 0°C ice-water bath, after the dropwise addition is completed, heat to 40°C, and stir the mixture at a constant temperature for 10 hours to obtain a reaction product c; the amount ratio of the reaction product 2, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01 5 mol: 1 35 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 35 mL; the amount ratio of the mixed solution a to the mixed solution b is 140 mL: 40 mL;
[0057] Step A4: Add glycidyl methacrylate and reaction product c into a three-necked flask, start stirring, slowly heat up to 62° C., slowly add potassium persulfate solution into the flask within 20 min, stir and react at constant temperature for 5 h, then heat up to 66° C., continue stirring and react for 30 min, and cool to room temperature to obtain an acrylic acid ester copolymer; the dosage ratio of glycidyl methacrylate, reaction product c, and potassium persulfate solution is 0.17 mol: 0.20 mol: 40 mL, and the concentration of potassium persulfate solution is 0.014 g / mL.
[0058] Example 4
[0059] An antioxidant, the preparation of which comprises the following steps:
[0060] Step B1: adding 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile to tetrahydrofuran, starting stirring, adding Raney nickel and Pd / C, introducing hydrogen, stirring and reacting at normal pressure for 48 hours, to obtain reaction product a; the amount ratio of 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 70 mL: 0.01 mol: 0.01 mol;
[0061] Step B2: Add the reaction product a, 4-bromo-3-nitrophenyl thiocyanate (supplier: Nanjing Shizhou Biotechnology Co., Ltd.) and methanol into a flask, add 2-dicyclohexylphospho-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and react with stirring at 80°C under nitrogen protection for 4 hours, and vacuum dry at 50°C to obtain the reaction product b; the amount ratio of the reaction product a, 4-bromo-3-nitrophenyl thiocyanate, methanol, 2-dicyclohexylphospho-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.12 mol: 90 mL: 0.0020 g: 0.0020 g: 0.20 mol;
[0062] Step B3: Add the reaction product b to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under normal pressure with stirring for 48 hours to obtain the reaction product c; the amount ratio of the reaction product b, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 110 mL: 0.04 mol: 0.040 mol;
[0063] Step B4: Add mesoporous titanium dioxide and reaction product c to ethanol, and then stir under vacuum for 6 hours. After the reaction is completed, centrifuge and dry to obtain the loaded product; add the loaded product to deionized water, stir for 10 minutes, add sodium hexametaphosphate, continue stirring and adjust the pH of the system to alkaline, then stir vigorously and heat to 80°C, adjust the pH of the system to 5, then slowly add sodium aluminate solution, stir for 30 minutes, adjust the pH to 7.0, filter, wash with water, and dry to obtain an antioxidant; the dosage ratio of mesoporous titanium dioxide, reaction product c, and ethanol is 0.5g:3g:60mL, and the volume fraction of ethanol is 95%; the dosage ratio of the loaded product, sodium hexametaphosphate, and sodium aluminate solution is 18g:50mL:15mL, and the concentration of the sodium aluminate solution is 0.1g / mL.
[0064] Example 5
[0065] An antioxidant, the preparation of which comprises the following steps:
[0066] Step B1: adding 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile to tetrahydrofuran, starting stirring, adding Raney nickel and Pd / C, introducing hydrogen, stirring and reacting at normal pressure for 48 hours, to obtain reaction product a; the amount ratio of 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 75 mL: 0.01 mol: 0.013 mol;
[0067] Step B2: Add the reaction product a, 4-bromo-3-nitrophenyl thiocyanate (supplier: Nanjing Shizhou Biotechnology Co., Ltd.) and methanol into a flask, add 2-dicyclohexylphospho-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and react with stirring at 80°C under nitrogen protection for 4.5h, and vacuum dry at 50°C to obtain the reaction product b; the amount ratio of the reaction product a, 4-bromo-3-nitrophenyl thiocyanate, methanol, 2-dicyclohexylphospho-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06mol:0.12mol:95mL:0.0020g:0.0020g:0.23mol;
[0068] Step B3: Add the reaction product b to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under normal pressure with stirring for 48 hours to obtain the reaction product c; the amount ratio of the reaction product b, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 115 mL: 0.04 mol: 0.043 mol;
[0069] Step B4: Add mesoporous titanium dioxide and reaction product c to ethanol, and then stir under vacuum for 7 hours. After the reaction is completed, centrifuge and dry to obtain the loaded product; add the loaded product to deionized water, stir for 1.5 minutes, add sodium hexametaphosphate, continue stirring and adjust the pH of the system to alkaline, then stir vigorously and heat to 80°C, adjust the pH of the system to 5, then slowly add sodium aluminate solution, stir for 35 minutes, adjust the pH to 7.0, filter, wash with water, and dry to obtain an antioxidant; the dosage ratio of mesoporous titanium dioxide, reaction product c, and ethanol is 0.7g:4g:60mL, and the volume fraction of ethanol is 95%; the dosage ratio of the loaded product, sodium hexametaphosphate, and sodium aluminate solution is 19g:55mL:17mL, and the concentration of the sodium aluminate solution is 0.1g / mL.
[0070] Example 6
[0071] An antioxidant, the preparation of which comprises the following steps:
[0072] Step B1: adding 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile to tetrahydrofuran, starting stirring, adding Raney nickel and Pd / C, introducing hydrogen, stirring and reacting at normal pressure for 48 hours, to obtain reaction product a; the amount ratio of 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 80 mL: 0.01 mol: 0.015 mol;
[0073] Step B2: Add the reaction product a, 4-bromo-3-nitrophenyl thiocyanate (supplier: Nanjing Shizhou Biotechnology Co., Ltd.) and methanol into a flask, add 2-dicyclohexylphospho-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and react with stirring at 80°C under nitrogen protection for 5 hours, and vacuum dry at 50°C to obtain the reaction product b; the amount ratio of the reaction product a, 4-bromo-3-nitrophenyl thiocyanate, methanol, 2-dicyclohexylphospho-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.12 mol: 100 mL: 0.0020 g: 0.0020 g: 0.25 mol;
[0074] Step B3: Add the reaction product b to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under normal pressure with stirring for 48 hours to obtain the reaction product c; the amount ratio of the reaction product b, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 120 mL: 0.04 mol: 0.045 mol;
[0075] Step B4: add mesoporous titanium dioxide and reaction product c to ethanol, and then stir under vacuum for 8 hours. After the reaction is completed, centrifuge and dry to obtain the loaded product; add the loaded product to deionized water, stir for 20 minutes, add sodium hexametaphosphate, continue stirring and adjust the pH of the system to alkaline, then stir vigorously and heat to 80°C, adjust the pH of the system to 6, then slowly add sodium aluminate solution, stir for 40 minutes, adjust the pH to 7.0, filter, wash with water, and dry to obtain an antioxidant; the dosage ratio of mesoporous titanium dioxide, reaction product c, and ethanol is 1g:5g:60mL, and the volume fraction of ethanol is 95%; the dosage ratio of the loaded product, sodium hexametaphosphate, and sodium aluminate solution is 20g:60mmL:20mL, and the concentration of the sodium aluminate solution is 0.1g / mL.
[0076] Example 7
[0077] A coating for building protection, comprising the following raw materials in parts by weight: 40 parts of acrylic copolymer, 5 parts of film-forming aid, 15 parts of pigment, 10 parts of filler, 0.3 parts of wetting agent, 0.4 parts of dispersant, 0.8 parts of thickener, 0.2 parts of defoamer, 0.3 parts of leveling agent, 1.0 parts of antioxidant and 30 parts of water; the film-forming aid is propylene glycol methyl ether acetate, the pigment is titanium dioxide, the filler is hollow glass microspheres, the wetting agent is fatty alcohol polyoxyethylene ether (supplier: Xingtai Xinlan Technology Co., Ltd.), the dispersant is polyacrylic acid sodium salt dispersant, the thickener is hydroxyethyl cellulose, the defoamer is emulsified silicone oil (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd.), and the leveling agent is polyether modified polysiloxane;
[0078] The preparation of the building protective coating comprises the following steps:
[0079] Step S1: Deionized water, defoamer, dispersant and wetting agent are placed in a dispersion tank, stirred at a speed of 500 r / min for 10 min, and then pigment and filler are added, and stirred at a speed of 1200 r / min for 20 min to obtain a mixed system;
[0080] Step S2: adjusting the rotation speed to 500 r / min, adding the acrylic copolymer obtained in Example 1, the film-forming aid, the thickener, the defoamer, the leveling agent, and the antioxidant obtained in Example 4 to the obtained mixed system, stirring for 10 minutes, and obtaining a building protective coating; the weight ratio of the defoamer added in step S1 and step S2 is 1:1, and the sum of the weights of the defoamers added in step S1 and step S2 is the total amount of the defoamer.
[0081] Example 8
[0082] A coating for building protection, comprising the following raw materials in parts by weight: 50 parts of acrylic copolymer, 6 parts of film-forming aid, 17 parts of pigment, 13 parts of filler, 0.4 parts of wetting agent, 0.6 parts of dispersant, 0.9 parts of thickener, 0.4 parts of defoamer, 0.4 parts of leveling agent, 1.3 parts of antioxidant and 35 parts of water; the film-forming aid is propylene glycol methyl ether acetate, the pigment is titanium dioxide, the filler is hollow glass microspheres, the wetting agent is fatty alcohol polyoxyethylene ether (supplier: Xingtai Xinlan Technology Co., Ltd.), the dispersant is polyacrylic acid sodium salt dispersant, the thickener is hydroxyethyl cellulose, the defoamer is emulsified silicone oil (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd.), and the leveling agent is polyether modified polysiloxane;
[0083] The preparation of the building protective coating comprises the following steps:
[0084] Step S1: Deionized water, defoamer, dispersant and wetting agent are placed in a dispersion tank, stirred at a speed of 550 r / min for 13 min, and then pigment and filler are added, and stirred at a speed of 1250 r / min for 23 min to obtain a mixed system;
[0085] Step S2: adjusting the rotation speed to 550 r / min, adding the acrylic copolymer obtained in Example 2, the film-forming aid, the thickener, the defoamer, the leveling agent, and the antioxidant obtained in Example 5 to the obtained mixed system, stirring for 12 minutes, and obtaining a building protective coating; the weight ratio of the defoamer added in step S1 and step S2 is 1:1, and the sum of the weights of the defoamers added in step S1 and step S2 is the total amount of the defoamer.
[0086] Example 9
[0087] A coating for building protection, comprising the following raw materials in parts by weight: 60 parts of acrylate copolymer, 7 parts of film-forming aid, 20 parts of pigment, 15 parts of filler, 0.5 parts of wetting agent, 0.8 parts of dispersant, 1.0 parts of thickener, 0.6 parts of defoamer, 0.5 parts of leveling agent, 1.5 parts of antioxidant and 40 parts of water; the film-forming aid is propylene glycol methyl ether acetate, the pigment is titanium dioxide, the filler is hollow glass microspheres, the wetting agent is fatty alcohol polyoxyethylene ether (supplier: Xingtai Xinlan Technology Co., Ltd.), the dispersant is polyacrylic acid sodium salt dispersant, the thickener is hydroxyethyl cellulose, the defoamer is emulsified silicone oil (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd.), and the leveling agent is polyether modified polysiloxane;
[0088] The preparation of the building protective coating comprises the following steps:
[0089] Step S1: Deionized water, defoamer, dispersant and wetting agent are placed in a dispersion tank, stirred at a speed of 600 r / min for 15 min, and then pigment and filler are added, and stirred at a speed of 1300 r / min for 25 min to obtain a mixed system;
[0090] Step S2: adjusting the rotation speed to 600 r / min, adding the acrylic copolymer obtained in Example 3, the film-forming aid, the thickener, the defoamer, the leveling agent, and the antioxidant obtained in Example 6 to the obtained mixed system, stirring for 15 minutes, and obtaining a building protective coating; the weight ratio of the defoamer added in step S1 and step S2 is 1:1, and the sum of the weights of the defoamers added in step S1 and step S2 is the total amount of the defoamer.
[0091] Comparative Example 1
[0092] This comparative example is a commercially available polyacrylate coating for building protection.
[0093] Comparative Example 2
[0094] Compared with Example 9, the acrylic acid ester copolymer was replaced with poly(glycidyl methacrylate), and the rest was exactly the same as Example 9 to prepare a building protective coating.
[0095] Comparative Example 3
[0096] Compared with Example 9, the antioxidant was replaced with the loaded product in Example 6, and the rest was exactly the same as Example 9 to prepare a building protective coating.
[0097] The effect of the building protective coating prepared by the present invention is further tested below, and the test results are as follows.
[0098] In order to test the building protective coating prepared by the present invention, the waterproofness of the coating was measured according to GB / T1733-1993 "Determination of water resistance of paint film"; the flame retardant time was measured according to GB12441-2018 "Finishing fire retardant coating", and the total smoke release was measured by cone calorimeter; the artificial aging test was performed according to GB / T1865-2009 "Artificial weathering and artificial radiation exposure of paints and varnishes to filtered xenon arc radiation", and the phenomena were recorded. The results are recorded in Table 1;
[0099] Table 1: Test results
[0100]
[0101]
[0102] According to the data in Table 1, compared with Example 1, it can be seen that the building protection coating prepared by the present invention has better water resistance, aging resistance and flame retardant and smoke suppression performance compared with the commercially available building protection polyacrylate coating. Compared with Comparative Example 2, Example 9 shows that the introduction of sodium sulfonate group and phosphoramide structure significantly improves the flame retardant and smoke suppression performance of the coating. Compared with Comparative Example 3, Example 9 shows that after the mesoporous titanium dioxide with small molecules loaded by hydrated alumina coating can better play the role of ultraviolet shielding, and synergistically improve the aging resistance of the coating with thioether and hindered phenol.
[0103] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A coating for building protection, characterized in that: The invention comprises the following raw materials in parts by weight: 40-60 parts of acrylic copolymer, 5-7 parts of film-forming aid, 15-20 parts of pigment, 10-15 parts of filler, 0.3-0.5 parts of wetting agent, 0.4-0.8 parts of dispersant, 0.8-1.0 parts of thickener, 0.2-0.6 parts of defoamer, 0.3-0.5 parts of leveling agent, 1.0-1.5 parts of antioxidant and 30-40 parts of water; The preparation of the acrylic acid ester copolymer comprises the following steps: Step A1: Add dimethylphosphoryl chloride to toluene, then add sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate, stir at 0-5°C for 2 hours, then heat to 40-50°C, reflux at constant temperature and stir for 1 hour, filter, extract and dry to obtain reaction product 1; Step A2: Add the reaction product 1 and ethyl acetate into a three-necked flask, heat to 45-55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1-1.5h to obtain the reaction product 2; Step A3: Add the reaction product 2, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, and stir the mixture at a constant temperature for 10 hours to obtain a reaction product c; Step A4: Add glycidyl methacrylate and reaction product c into a three-necked flask, start stirring, slowly heat up to 58-62°C, slowly add potassium persulfate solution into the flask within 20 minutes, stir and react at a constant temperature for 4-5 hours, then heat up to 64-66°C, continue stirring and reacting for 30 minutes, and cool to room temperature to obtain an acrylic copolymer.
2. A building protective coating according to claim 1, characterized in that: In step A1, the usage ratio of dimethylphosphoryl chloride, toluene, and sodium 5-amino-4-methoxy-2-nitrobenzenesulfonate is 0.1 mol: 100-110 mL: 0.1 mol; in step A2, the usage ratio of reaction product 1, ethyl acetate, and sodium dithionite is 0.1 mol: 120-130 mL: 0.1-0.15 mol.
3. A building protective coating according to claim 1, characterized in that: In step A3, the dosage ratio of reaction product 2, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01 5 mol: 125-1 35 mL; the dosage ratio of methacryloyl chloride and dimethyl sulfoxide is 0.1 mol: 25-35 mL; the dosage ratio of mixed solution a and mixed solution b is 130-140 mL: 30-40 mL; in step A4, the dosage ratio of glycidyl methacrylate, reaction product c and potassium persulfate solution is 0.17 mol: 0.20 mol: 35-40 mL, and the concentration of potassium persulfate solution is 0.014 g / mL.
4. The building protective coating according to claim 1, characterized in that: The preparation of the antioxidant comprises the following steps: Step B1: Add 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under normal pressure with stirring for 48 hours to obtain reaction product a; Step B2: Add the reaction product a, 4-bromo-3-nitrophenylthiocyanate and methanol into a flask, add 2-dicyclohexylphosphino-2'-4'-6'-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate, reflux and stir at 80° C. under nitrogen protection for 4-5 hours, and vacuum dry at 50° C. to obtain the reaction product b; Step B3: Add the reaction product b to tetrahydrofuran, start stirring, add Raney nickel and Pd / C, introduce hydrogen, and react under stirring at normal pressure for 48 hours to obtain the reaction product c; Step B4: adding mesoporous titanium dioxide and reaction product c to ethanol, and then stirring for 6-8 hours under vacuum conditions. After the reaction is completed, centrifuging and drying are performed to obtain the loaded product; Add the loaded product to deionized water, stir for 10-20 minutes, add sodium hexametaphosphate, continue stirring and adjust the pH of the system to alkaline, then stir vigorously and heat to 80°C, adjust the pH of the system to 5-6, then slowly add sodium aluminate solution, stir for 30-40 minutes, adjust the pH to 7.0, filter, wash with water, and dry to obtain the antioxidant.
5. A building protective coating according to claim 4, characterized in that: In step B1, the usage ratio of 3,5-di-tert-butyl-4-hydroxybenzeneacetonitrile, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 70-80 mL: 0.01mol:0.01-0.015mol.
6. A building protective coating according to claim 4, characterized in that: In step B2, the usage ratio of reaction product a, 4-bromo-3-nitrophenyl thiocyanate, methanol, 2-dicyclohexylphospho-2′-4′-6′-triisopropylbiphenyl, tris(dibenzylideneacetone)dipalladium and potassium carbonate is 0.06 mol: 0.12 mol: 90-100 mL: 0.0020 g: 0.0020 g: 0.20-0.25 mol.
7. A building protective coating according to claim 4, characterized in that: In step B3, the dosage ratio of reaction product b, tetrahydrofuran, Raney nickel and Pd / C is 0.1 mol: 110-120 mL: 0.04 mol: 0.040-0.045 mol; in step B4, the dosage ratio of mesoporous titanium dioxide, reaction product c and ethanol is 0.5-1 g: 3-5 g: 60 mL, and the volume fraction of ethanol is 95%; the dosage ratio of loaded product, sodium hexametaphosphate and sodium aluminate solution is 18-20 g: 50-60 mL: 15-20 mL, and the concentration of sodium aluminate solution is 0.1 g / mL.
8. The building protective coating according to claim 1, characterized in that: The film-forming aid is propylene glycol methyl ether acetate, the pigment is titanium dioxide, the filler is hollow glass microspheres, the wetting agent is fatty alcohol polyoxyethylene ether, the dispersant is polyacrylic acid sodium salt dispersant, the thickener is hydroxyethyl cellulose, the defoamer is emulsified silicone oil, and the leveling agent is polyether modified polysiloxane.
9. The method for preparing a building protective coating according to claim 1, characterized in that: The steps include: Step S1: Deionized water, defoamer, dispersant and wetting agent are placed in a dispersion tank, stirred at a speed of 500-600 r / min for 10-15 min, and then pigment and filler are added, and stirred at a speed of 1200-1300 r / min for 20-25 min to obtain a mixed system; Step S2: adjusting the rotation speed to 500-600 r / min, adding acrylic copolymer, film-forming aid, thickener, defoamer, leveling agent and antioxidant to the obtained mixed system, stirring for 10-15 minutes, and obtaining a coating for building protection.
10. The method for preparing a building protective coating according to claim 9, characterized in that: The weight ratio of the defoaming agent added in step S1 and step S2 is 1:1, and the sum of the weights of the defoaming agent added in step S1 and step S2 is the total amount of the defoaming agent.
Citation Information
Patent Citations
Flame-retardant reflection insulation paint and preparation method thereof
CN103073963A
Loaded rubber anti-aging agent and preparation method and application thereof
CN105670040A
Flame-retardant water-based acrylic resin and preparation method thereof
CN109810216A
Silica-encapsulated loading mesoporous silicon and preparation method and application thereof
CN116459168A
Anti-yellowing high-glossiness artistic coating
CN117534993A