Method for rapidly evaluating phosphate fire-resistant oil performance based on metal catalytic oxidation
Through the synergistic action of the polymetal catalyst and oxygen, the deterioration of phosphate fuel resistance is accelerated, and the problem of long test cycles in the prior art is solved, and the rapid and accurate evaluation of phosphate fuel resistance performance is achieved.
Patent Information
- Application Number
- CN202411301719.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the test cycle of phosphate fuel resistance performance evaluation is too long and performance cannot be accurately evaluated in time.
The synergistic action of polymetallic catalysts and oxygen is used to accelerate the formation of free radicals in the presence of oxygen through anhydrous copper nitrate and anhydrous nitrate catalysts, and rapidly deteriorate the phosphate fuel-resistant oil, thereby evaluating its performance in a short time.
It significantly shortens the detection cycle, improves the detection speed and accuracy, and can accurately evaluate the stable performance of phosphate fuel resistance in a short period of time.
Smart Images

Figure BDA0005047856690000091 
Figure BDA0005047856690000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of phosphate fire-resistant oils, and in particular relates to a method for quickly evaluating the performance of phosphate fire-resistant oils based on metal catalytic oxidation. Background Art
[0002] Triaryl phosphates are important raw materials in the chemical production process. In the field of polymers, triaryl phosphates are often used as flame retardants and additives for materials such as plastics and synthetic rubbers, which can significantly improve the flame retardant properties of plastics and rubber products. In the field of power, triaryl phosphates, as the main component of phosphate fire-resistant oils, are often used in the speed control system of power generation steam turbines, playing an important role in ensuring the normal, safe and stable operation of steam turbine units. However, due to the huge difference in the use environment of triaryl phosphates in the power field and the plastic products field, the requirements for phosphates in the two are also different. The polymer field requires triaryl phosphates to have a higher auto-ignition point. In the field of power, the auto-ignition point, flash point, kinematic viscosity and foam properties of triaryl phosphates used for fire-resistant oils must not only meet the requirements of the DL / T571 "Guidelines for the Operation and Maintenance of Phosphate Fire-Resistant Oils for Power Plants" standard, but also have excellent stability.
[0003] At present, the main methods for evaluating the stability of phosphate ester fire-resistant oils are the oxidation stability determination method specified in the standard EN 14832 "Petroleum and related products-Determination of the oxidation stability and corrosivity of fire-resistant phosphate ester fluids" and the hydrolysis stability determination method specified in the standard EN14833 "Petroleum and related products-Determination of the hydrolytic stability of fire-resistant phosphate ester fluids". The combination of the two methods can measure the oxidation resistance and hydrolysis resistance of phosphate ester fire-resistant oils to a certain extent. In addition, the closed cup aging method of the standard DL / T1705 "Closed cup aging determination method for phosphate ester fire-resistant oils" can also accurately evaluate the stability of phosphate ester fire-resistant oils.
[0004] However, the above methods have the disadvantage that the required test period is too long and cannot accurately evaluate the performance of phosphate ester fire retardant oils in a timely manner. For example, the time specified in EN 14832 and DL / T1705 is 164 hours, and the time specified in EN 14833 is 96 hours. Summary of the invention
[0005] The purpose of the present invention is to solve the problem of long test cycle for evaluating the performance of phosphate ester fire-resistant oil in the above-mentioned prior art, and to provide a method for quickly and accurately evaluating the performance of phosphate ester fire-resistant oil, which can effectively shorten the detection cycle of the prior art and has the characteristics of fast detection speed and high accuracy.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for quickly evaluating the performance of phosphate fire-resistant oil based on metal catalytic oxidation, which specifically comprises the following steps:
[0008] S1: dissolving anhydrous copper nitrate and anhydrous nickel nitrate in water, mixing and stirring, and fully dissolving to obtain a solution;
[0009] S2: adding a dilute alkali solution to the solution until the solution is alkaline, stirring, standing and filtering, and then washing the obtained solid with an organic solvent and water until the pH value is 7; drying and grinding into powder, calcining, and cooling to obtain a multi-metal catalyst;
[0010] S3: Add multi-metal catalyst and water to phosphate fire-resistant oil, introduce air into the phosphate fire-resistant oil, heat and stir, filter to obtain treated oil sample after cooling, detect acid value and resistivity of the oil sample, and evaluate the performance of the oil sample.
[0011] Preferably, the molar ratio of copper nitrate to nickel nitrate is 1:(1-5).
[0012] Preferably, the dilute alkali solution is a sodium hydroxide solution or a potassium hydroxide solution with a concentration of 0.5% to 2%.
[0013] Preferably, the alkaline solution in S2 means that the pH of the solution is 8-10.
[0014] Preferably, the stirring time in S2 is 0.5 to 1.5 h.
[0015] Preferably, the calcination conditions in S2 are: calcination at 300-600° C. for 3-5 hours.
[0016] Preferably, the mass of the multi-metal catalyst in S3 is 1% to 5% of the mass of the phosphate fire-resistant oil.
[0017] Preferably, the mass of the water in S3 is 0.5% to 3% of the mass of the phosphate fire-resistant oil.
[0018] Preferably, the flow rate of the introduced air is 500-1000 mL / min.
[0019] Preferably, the heating temperature in S3 is 120-150°C.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The prior art uses a copper wire catalyst to catalyze the degradation of phosphate fire-resistant oil at a certain temperature, but the number of free radicals generated within a certain period of time is small, and the degradation rate of phosphate fire-resistant oil is slow. The present invention uses a multi-metal catalyst and the introduction of oxygen to greatly accelerate the generation rate of free radicals, and a large number of free radicals can be generated in a short time, accelerating the degradation of unstable triaryl phosphates in phosphate fire-resistant oil, thereby achieving the purpose of quickly evaluating the performance of phosphate fire-resistant oil in a short time. DETAILED DESCRIPTION
[0022] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0023] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0024] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0025] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0026] The present invention utilizes the synergistic effect of a multi-metal catalyst and oxygen to significantly accelerate the generation process of free radicals. Through the multi-metal catalyst (including anhydrous copper nitrate and anhydrous nickel nitrate), in the presence of oxygen, the multi-metal catalyst can efficiently catalyze the dissociation of oxygen molecules to generate a large number of free radicals, thereby accelerating the degradation of unstable triaryl phosphates in phosphate fire-resistant oils, thereby achieving the purpose of quickly evaluating the performance of phosphate fire-resistant oils in a short time.
[0027] The present invention provides a method for quickly evaluating the performance of phosphate fire-resistant oil based on metal catalytic oxidation, comprising the following steps:
[0028] S1: dissolving anhydrous copper nitrate and anhydrous nickel nitrate in water, mixing and stirring, and fully dissolving to obtain a solution;
[0029] S2: slowly adding a dilute alkali solution dropwise to the solution until the solution is alkaline, stirring, standing and filtering, and then washing the obtained solid with an organic solvent and water until the pH value is 7; drying and grinding into powder, calcining, and cooling to obtain a multi-metal catalyst;
[0030] S3: Add multi-metal catalyst and water to phosphate fire-resistant oil, introduce air into the phosphate fire-resistant oil, heat and stir, filter to obtain treated oil sample after cooling, detect acid value and resistivity of the oil sample, and evaluate the performance of the oil sample.
[0031] Among them, the water is preferably deionized water; the molar ratio of copper nitrate to nickel nitrate is 1:(1-5), and the use of anhydrous copper nitrate and anhydrous nickel nitrate as raw materials ensures the high purity of the catalyst precursor, which is beneficial to the activity of the subsequent catalyst; the dilute alkali solution is a sodium hydroxide solution or a potassium hydroxide solution with a concentration of 0.5% to 2%.
[0032] The solution in S2 is alkaline, which means that the pH of the solution is 8-10. The pH of 8-10 ensures the smooth progress of the precipitation process, which is conducive to the formation of a catalyst precursor with a stable structure and uniform particle size; the organic solvent is methanol, ethanol, propanol, styrene and ethylene glycol ether, etc.
[0033] The stirring time in S2 is 0.5 to 1.5 hours, and the standing time is 8 to 16 hours; the drying temperature in S2 is 100 to 150°C; the calcination conditions are: calcination at 300 to 600°C for 3 to 5 hours. The drying and calcination promote the crystallization and phase change of the catalyst, and enhance its catalytic activity and stability.
[0034] The mass of the multi-metal catalyst in S3 is 1% to 5% of the mass of the phosphate fire-resistant oil; the mass of the water in S3 is 0.5% to 3% of the mass of the phosphate fire-resistant oil.
[0035] The flow rate of the introduced air is 500-1000 mL / min; the heating temperature in S3 is 120-150°C.
[0036] Example 1
[0037] Take two different phosphate fire-resistant oils, A and B, and perform the following steps respectively:
[0038] Take 1.88g (0.01mol) of anhydrous copper nitrate and 1.83g (0.01mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 0.5% sodium hydroxide solution drop by drop until the pH of the solution is 9, and continue stirring for 0.5h. After stirring, place the solution in an oven and let it stand for 12h, filter, and wash the obtained solid with methanol and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 120°C, grind it into powder and place it in a muffle furnace, calcine it at 400°C for 3h, and obtain a multi-metal catalyst after cooling.
[0039] 2.00g of multi-metal catalyst and 1.00g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 500mL / min, and stirred at 120°C for 1h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0040] Example 2
[0041] Take two different phosphate fire-resistant oils, A and B, and perform the following steps respectively:
[0042] Take 1.88g (0.01mol) of anhydrous copper nitrate and 3.66g (0.02mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 1% sodium hydroxide solution drop by drop until the pH of the solution is 9, and continue stirring for 1h. After stirring, place the solution in an oven and let it stand for 12h, filter, and wash the obtained solid with methanol and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 120°C, grind it into powder and place it in a muffle furnace, calcine it at 400°C for 4h, and obtain a multi-metal catalyst after cooling.
[0043] 3.00g of multi-metal catalyst and 1.50g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 800mL / min, and stirred at 135°C for 1h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0044] Example 3
[0045] Take two different phosphate fire-resistant oils, A and B, and perform the following steps respectively:
[0046] Take 1.88g (0.01mol) of anhydrous copper nitrate and 9.15g (0.05mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 1% sodium hydroxide solution drop by drop until the pH of the solution is 10, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 12h, filter, and wash the obtained solid with methanol and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 120°C, grind it into powder and place it in a muffle furnace, calcine it at 400°C for 5h, and obtain a multi-metal catalyst after cooling.
[0047] 5.00g of multi-metal catalyst and 3.00g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 1000mL / min. The mixture was stirred at 150°C for 1h. Then, the introduction of air and heating were stopped, and the treated oil sample was filtered after cooling. The acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0048] Example 4
[0049] Take 1.88g (0.01mol) of anhydrous copper nitrate and 5.49g (0.03mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 1.5% sodium hydroxide solution drop by drop until the pH of the solution is 10, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 8h, filter, and wash the obtained solid with ethanol and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 100°C, grind it into powder and place it in a muffle furnace, calcine it at 300°C for 5h, and obtain a multi-metal catalyst after cooling.
[0050] 1.00g of multi-metal catalyst and 0.50g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 500mL / min, and stirred at 130°C for 1h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0051] Example 5
[0052] Take 1.88g (0.01mol) of anhydrous copper nitrate and 7.32g (0.04mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 2% sodium hydroxide solution drop by drop until the pH of the solution is 8, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 9h, filter, and wash the obtained solid with propanol and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 110°C, grind it into powder and place it in a muffle furnace, calcine it at 350°C for 5h, and obtain a multi-metal catalyst after cooling.
[0053] 1.50g of multi-metal catalyst and 0.50g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 600mL / min, and stirred at 140°C for 1h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0054] Example 6
[0055] Take 1.88g (0.01mol) of anhydrous copper nitrate and 9.15g (0.05mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 0.5% potassium hydroxide solution drop by drop until the pH of the solution is 8, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 10h, filter, and wash the obtained solid with styrene and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 130°C, grind it into powder and place it in a muffle furnace, calcine it at 450°C for 4h, and obtain a multi-metal catalyst after cooling.
[0056] 2.50g of multi-metal catalyst and 1.00g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 700mL / min, and stirred at 145°C for 1h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0057] Example 7
[0058] Take 1.88g (0.01mol) of anhydrous copper nitrate and 9.15g (0.05mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 1% potassium hydroxide solution drop by drop until the pH of the solution is 9, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 11h, filter, and wash the obtained solid with styrene and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 140°C, grind it into powder and place it in a muffle furnace, calcine it at 500°C for 4h, and obtain a multi-metal catalyst after cooling.
[0059] 3.00g of multi-metal catalyst and 1.50g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 800mL / min, and stirred at 150°C for 2h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0060] Example 8
[0061] Take 1.88g (0.01mol) of anhydrous copper nitrate and 9.15g (0.05mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 1.5% potassium hydroxide solution drop by drop until the pH of the solution is 9, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 13h, filter, and wash the obtained solid with ethylene glycol ether and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 150°C, grind it into powder and place it in a muffle furnace, calcine it at 550°C for 3h, and obtain a multi-metal catalyst after cooling.
[0062] 3.50g of multi-metal catalyst and 2.00g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 900mL / min, and stirred at 150°C for 3h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0063] Example 9
[0064] Take 1.88g (0.01mol) of anhydrous copper nitrate and 9.15g (0.05mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 2% potassium hydroxide solution drop by drop until the pH of the solution is 10, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 15h, filter, and wash the obtained solid with ethylene glycol ether and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 130°C, grind it into powder and place it in a muffle furnace, calcine it at 550°C for 3h, and obtain a multi-metal catalyst after cooling.
[0065] 4.00g of multi-metal catalyst and 2.50g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 900mL / min, and stirred at 120°C for 1h. Subsequently, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling, and the acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0066] Example 10
[0067] Take 1.88g (0.01mol) of anhydrous copper nitrate and 9.15g (0.05mol) of anhydrous nickel nitrate and dissolve them in deionized water, mix and stir, fully dissolve, slowly add a 2% potassium hydroxide solution drop by drop until the pH of the solution is 10, and continue stirring for 1.5h. After stirring, place the solution in an oven and let it stand for 16h, filter, and wash the obtained solid with methanol and deionized water until the pH of the aqueous solution is 7. Subsequently, place the solid in an oven and dry it at 140°C, grind it into powder and place it in a muffle furnace, calcine it at 600°C for 3h, and obtain a multi-metal catalyst after cooling.
[0068] 4.50g of multi-metal catalyst and 3.00g of deionized water were added to 100.00g of phosphate fire-resistant oil, and air was introduced into the phosphate fire-resistant oil at a rate of 1000mL / min. The mixture was stirred at 140°C for 1h. Then, the introduction of air was stopped, the heating was suspended, and the treated oil sample was filtered after cooling. The acid value and resistivity of the oil sample were tested to evaluate the performance of the oil sample.
[0069] In order to measure the accuracy of this method, the closed cup aging method was used to age the two different phosphate ester fire-resistant oils A and B in Examples 1 to 10 and the two different phosphate ester fire-resistant oils A and B before treatment, and the acid value and resistivity were tested. The specific operation process is as follows:
[0070] First, the water content of phosphate fire-resistant oil was adjusted to 800 mg / L±50 mg / L. Then, 200.0 g of phosphate fire-resistant oil was placed in a conical flask, the cleaned spiral copper wire was placed in the conical flask, and a ground stopper was put on. Then, the conical flask was placed in an oven at 115°C±1°C, and aged for 164 hours in the oven. After the aging, the conical flask containing the sample was taken out, and after cooling to room temperature, the acid value and resistivity of the oil sample were detected. The performance test results of Examples 1 to 10 and two different phosphate fire-resistant oils A and B after closed-end aging are shown in Table 1.
[0071] Table 1 Performance test data of phosphate fire-resistant oil obtained by Examples 1 to 10 and closed-end aging
[0072]
[0073]
[0074] As can be seen from the above table, in the closed cup aging test method, the changes in the acid value and resistivity of oil sample A are less than those of oil sample B, indicating that the stability of sample A is better than that of sample B. The acid value and resistivity change trends of oil samples A and B in Examples 1 to 10 of the present invention are consistent with those of the closed cup aging method, that is, the acid value increases and the resistivity decreases, and the acid value and resistivity changes of oil sample A are both less than those of oil sample B, which also indicates that the stability of sample A is better than that of sample B. That is, the results obtained by the metal catalytic oxidation method are consistent with those obtained by the prior art method, and the detection cycle is greatly shortened, which significantly reduces the time required for the test.
[0075] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for rapidly evaluating the performance of phosphate fire-resistant oils based on metal catalytic oxidation, characterized in that: The specific steps include: S1: dissolving anhydrous copper nitrate and anhydrous nickel nitrate in water, mixing and stirring, and fully dissolving to obtain a solution; S2: adding a dilute alkali solution to the solution until the solution is alkaline, stirring, standing and filtering, and then washing the obtained solid with an organic solvent and water until the pH value is 7; drying and grinding into powder, calcining, and cooling to obtain a multi-metal catalyst; S3: Add multi-metal catalyst and water to phosphate fire-resistant oil, introduce air into the phosphate fire-resistant oil, heat and stir, filter to obtain treated oil sample after cooling, detect acid value and resistivity of the oil sample, and evaluate the performance of the oil sample.
2. The method for rapidly evaluating the performance of phosphate ester fire-resistant oils based on metal catalytic oxidation according to claim 1, characterized in that: The molar ratio of the copper nitrate to the nickel nitrate is 1:(1-5).
3. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The dilute alkali solution is a sodium hydroxide solution or a potassium hydroxide solution with a concentration of 0.5% to 2%.
4. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The alkaline solution in S2 means that the pH of the solution is 8-10.
5. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The stirring time in S2 is 0.5 to 1.5 h.
6. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The calcination conditions in S2 are: calcination at 300-600° C. for 3-5 hours.
7. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The mass of the multi-metal catalyst in S3 is 1% to 5% of the mass of the phosphate fire-resistant oil.
8. The method for rapidly evaluating the performance of phosphate ester fire-resistant oils based on metal catalytic oxidation according to claim 1, characterized in that: The mass of the water in S3 is 0.5% to 3% of the mass of the phosphate fire-resistant oil.
9. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The flow rate of the introduced air is 500-1000 mL / min.
10. The method for rapidly evaluating the performance of phosphate ester fire-resistant oil based on metal catalytic oxidation according to claim 1, characterized in that: The heating temperature in S3 is 120-150°C.