Polyimide nano composite film and preparation method thereof

By cross-linking nanosheet fillers with metal ions on a nylon filter membrane, the method enhances mechanical strength and thermal conductivity of polyimide films, addressing the limitations of traditional films.

CN119236714APending Publication Date: 2025-01-03BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411523424.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2025-01-03

AI Technical Summary

Technical Problem

Traditional polyimide films have low inherent thermal conductivity and mechanical properties due to agglomeration of nanofillers and low orientation degree, making them unsuitable for high-performance applications.

Method used

A method involving mixing polyamic acid solution with nanosheet fillers containing oxygen-containing groups, pouring onto a nylon filter membrane soaked with metal ions, and thermal imidization to create a polyimide nanocomposite film with oriented nanofillers cross-linked by metal ions, enhancing mechanical strength and thermal conductivity.

Benefits of technology

The method produces a polyimide nanocomposite film with high mechanical strength and thermal conductivity, achieving strengths up to 390 MPa and thermal conductivity of 84.8 W/(mK) with 80wt% graphene oxide, surpassing conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119236714A_ABST
    Figure CN119236714A_ABST
Patent Text Reader

Abstract

The invention provides a polyimide nano composite film and a preparation method thereof, and relates to the technical field of polyimide materials. The preparation method comprises the following steps: mixing a polyamide acid solution with a nano filler to obtain a mixed dispersion liquid; pouring the mixed dispersion liquid on a nylon filter membrane infiltrated with metal ions, and drying to obtain the polyamide acid nano composite membrane on the surface of the nylon filter membrane. And carrying out thermal imidization on the polyamide acid nano-composite film to obtain the polyimide nano-composite film. According to the preparation method, the polyamide acid solution and the nano-filler are mixed, then the composite membrane is prepared in a metal ion cross-linking mode, shearing force generated in the spreading process of mixed dispersion liquid can induce orientation of nanosheets, metal ions infiltrated on the nylon filter membrane can cross-link the nano-filler firstly, and the oriented nanosheets are fixed in time. The polyimide nano-composite film which is high in nano-filler content, uniform and good in orientation can be prepared, and the polyimide nano-composite film has high mechanical strength and high heat-conducting property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyimide materials, and in particular to a polyimide nanocomposite film and a preparation method thereof. Background Art

[0002] Polyimide (PI) is usually first obtained by reacting dibasic acid anhydride and dibasic aromatic amine under mild conditions to obtain the precursor polyamic acid (PAA), and then obtained by gradual heating or chemical cyclization. PI has excellent mechanical properties, heat resistance, chemical resistance and other excellent properties, and has shown outstanding performance in many fields. The development of high-performance PI is of great significance to the development of high-tech industries.

[0003] In recent years, with the rapid development of electronic products and 5G communication technology, the heating problem has become more serious. PI has excellent flexibility and heat resistance, and is a potential material to replace traditional thermal conductive substrates. However, the common pure PI film has a low inherent thermal conductivity (<1W / (mK)), which is difficult to meet the requirements of practical applications. At present, this problem can be improved through molecular design or the addition of nanofillers.

[0004] Among them, in terms of adding nanofillers, common fillers are divided into carbon-based materials, such as graphene, graphene oxide, carbon nanotubes, etc., and ceramic-based materials, such as boron nitride. The traditional method of preparing PI nanocomposite films is mostly to simply blend PI and nanofillers in a solvent, and then obtain a film by casting or coating. In the film obtained by this method, the filler is easy to agglomerate, and the orientation degree is low, and the filler content is difficult to increase (<40wt%), so that the mechanical properties and thermal conductivity of the film are not up to expectations. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a polyimide nanocomposite film and a preparation method thereof. The preparation method provided by the present invention can prepare a polyimide nanocomposite film with high, uniform and well-oriented nanofiller content, and the obtained polyimide nanocomposite film has both high mechanical strength and high thermal conductivity.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a polyimide nanocomposite film, comprising the following steps:

[0008] The polyamic acid solution is mixed with a nanofiller to obtain a mixed dispersion; the nanofiller is a nanosheet filler having oxygen-containing groups on the surface;

[0009] The mixed dispersion is poured onto a nylon filter membrane soaked with metal ions, and after drying, a polyamic acid nanocomposite membrane is obtained on the surface of the nylon filter membrane;

[0010] The polyamic acid nanocomposite film is thermally imidized to obtain a polyimide nanocomposite film.

[0011] Preferably, the solid content of the polyamic acid solution is 10-20 wt %.

[0012] Preferably, the nanofiller comprises graphene oxide.

[0013] Preferably, the mass of the nanofiller in the mixed dispersion is 0 to 80% of the total solid mass in the mixed dispersion, and is not 0.

[0014] Preferably, the metal ions include one or more of monovalent metal ions, divalent metal ions and trivalent metal ions.

[0015] Preferably, the monovalent metal ions include sodium ions and / or potassium ions, the divalent metal ions include one or more of calcium ions, magnesium ions and copper ions, and the trivalent metal ions include iron ions.

[0016] Preferably, the nylon filter membrane impregnated with metal ions is obtained by dripping a solution of the metal ions onto the nylon filter membrane, and the concentration of the metal ions in the solution of the metal ions is 0.1 to 0.5 mol / L.

[0017] Preferably, the drying includes first drying and second drying in sequence, the first drying temperature is 80-120°C, the insulation time is 20-40 minutes, the second drying temperature is 200-230°C, and the insulation time is 20-40 minutes; after the first drying, the obtained film is peeled off the nylon filter membrane.

[0018] Preferably, the thermal imidization comprises a first stage and a second stage, wherein the temperature of the first stage is 300-330° C., the insulation time is 20-40 min, and the temperature of the second stage is 400-430° C., the insulation time is 90-120 min.

[0019] The present invention provides a polyimide nanocomposite film prepared by the preparation method described in the above technical solution. The polyimide nanocomposite film comprises a polyimide film and nanofillers doped in the polyimide film. The nanofillers are cross-linked by metal ions.

[0020] The invention provides a method for preparing a polyimide nanocomposite film, comprising the following steps: mixing a polyamic acid solution with a nanofiller (having an oxygen-containing group) to obtain a mixed dispersion; pouring the mixed dispersion onto a nylon filter membrane infiltrated with metal ions, drying, and obtaining a polyamic acid nanocomposite film on the surface of the nylon filter membrane; thermal imidization of the polyamic acid nanocomposite film to obtain a polyimide nanocomposite film. The invention mixes a polyamic acid solution with a nanofiller, pours the mixture onto a nylon filter membrane infiltrated with metal ions, and prepares a composite film by cross-linking metal ions. The shear force generated during the spreading process of the mixed dispersion induces the orientation of nanosheets. The metal ions infiltrated on the nylon filter membrane cross-link the nanofillers first, construct a first layer of cross-linked network, and timely fix the oriented nanosheets. In the process of drying and solvent volatilization, the nanofiller agglomeration can be significantly reduced, and a high degree of orientation can be maintained, so that the reinforcing effect of the nanofiller is fully exerted, and the content of the filler can be further increased, so as to obtain a polyimide nanocomposite film with high mechanical properties and high thermal conductivity.

[0021] The results of the embodiment show that the method of the present invention can prepare a uniform and flat polyimide nanocomposite film with nanofillers ranging from low concentration to high concentration (0-80wt%). The composite film containing 2.5wt% graphene oxide prepared by the method of the present invention has extremely high mechanical properties, strength of 390MPa, strain of 33%, and modulus of 4.1GPa; with the increase of graphene oxide content, the modulus of the composite film continues to increase, and the modulus of the composite film containing 80wt% graphene oxide is as high as 10.3GPa; in comparison, the strength of the pure polyimide film is 228MPa, the strain is 13%, and the modulus is 3.5GPa. In addition, the thermal conductivity of the composite film also increases significantly with the increase of graphene oxide content. The thermal conductivity of the composite film containing 80wt% graphene oxide can reach 84.8W / (mK), and the thermal conductivity of the composite films with different graphene oxide contents is also higher than that of the films obtained by other methods, such as casting and scraping. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The physical pictures of GO / PAA composite films with different GO contents in Example 1, Example 5 and Example 8 are shown in FIG. Figure 1 From left to right, they correspond to the GO / PAA composite films of Example 1, Example 5, and Example 8;

[0023] Figure 2 : are the tensile stress-strain curves of the GO / PI composite films with different GO contents prepared in Examples 1 to 8 and Comparative Example 1, Figure 2 a is the tensile stress-strain curve of GO / PI composite films with different GO contents, and b is the enlarged view of the first 2% strain in a;

[0024] Figure 3 is the in-plane thermal conductivity of the GO / PI composite films with different GO contents prepared in Examples 1 to 8 and Comparative Example 1;

[0025] Figure 4 The mechanical properties and thermal conductivity of the GO / PI composite film obtained in the embodiment of the present invention are compared with those of other PIs;

[0026] Figure 5 The scanning electron microscope (SEM) images of GO / PI composite films with different GO contents prepared in Example 1, Examples 3 to 8 and Comparative Example 1;

[0027] Figure 6 2D WAXS images of GO / PI composite films with different GO contents prepared in Example 1, Examples 2 to 6, Example 8 and Comparative Example 1;

[0028] Figure 7 The SEM images of xGO / PI' composite membranes with different GO contents prepared in Example 9;

[0029] Figure 8 This is the in-plane thermal conductivity of the xGO / PI' composite films with different GO contents prepared in Example 9. DETAILED DESCRIPTION

[0030] The present invention provides a method for preparing a polyimide nanocomposite film, comprising the following steps:

[0031] The polyamic acid solution is mixed with a nanofiller to obtain a mixed dispersion; the nanofiller is a nanosheet filler having oxygen-containing groups on the surface;

[0032] The mixed dispersion is poured onto a nylon filter membrane soaked with metal ions, and after drying, a polyamic acid nanocomposite membrane is obtained on the surface of the nylon filter membrane;

[0033] The polyamic acid nanocomposite film is thermally imidized to obtain a polyimide nanocomposite film.

[0034] In the present invention, unless otherwise specified, the raw materials involved are commercially available products well known in the art.

[0035] The present invention mixes the polyamic acid solution with the nano filler to obtain a mixed dispersion. In the present invention, the solid content of the polyamic acid solution is preferably 10 to 20 wt%.

[0036] The present invention has no special requirements on the source of the polyamic acid solution, and the polyamic acid solution can be prepared using commercially available products or a preparation method well known to those skilled in the art.

[0037] In an embodiment of the present invention, the preparation method of the polyamic acid solution includes: mixing dianhydride, diamine and organic solvent for polymerization reaction to obtain a polyamic acid solution. The present invention has no special requirements for the dianhydride and diamine, and the dianhydride and diamine well known to those skilled in the art can be used. Specifically, the dianhydride is such as 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and pyromellitic dianhydride (PMDA), and the diamine is such as 2-(4-aminophenyl)-5-aminobenzimidazole (BIA) and 4,4'-diaminodiphenyl ether (ODA). In the present invention, the molar ratio of the dianhydride and the diamine is preferably 1:1. In the present invention, the organic solvent is preferably N-methylpyrrolidone (NMP). In the present invention, the method of mixing the dianhydride, diamine and organic solvent is preferably: under a nitrogen atmosphere, the diamine is dissolved in an organic solvent, and then the dianhydride is added thereto, and then the organic solvent is added to make the solid content of the mixed solution 10 to 20wt%. In the present invention, the polymerization reaction temperature is preferably 20 to 30° C., the polymerization reaction time is preferably 4 to 6 hours, and the polymerization reaction is preferably carried out under stirring.

[0038] In the present invention, the nanofiller is a nanosheet filler having oxygen-containing groups on the surface, so that it can be cross-linked by metal ions. In the present invention, the nanofiller preferably includes graphene oxide (GO). In an embodiment of the present invention, the lateral size of the graphene oxide is preferably 3 to 5 μm. In the present invention, the nanofiller is preferably added in the form of a nanofiller dispersion, and the dispersion medium of the nanofiller dispersion is preferably N-methylpyrrolidone (NMP). In an embodiment of the present invention, the concentration of the nanofiller dispersion is preferably 3 mg / mL. The present invention has no special requirements for the mixing method of the polyamic acid solution and the nanofiller, and they can be mixed evenly using a mixing method well known to those skilled in the art.

[0039] In the present invention, the mass of the nanofiller in the mixed dispersion is preferably 0-80% (not 0) of the total solid mass in the mixed dispersion, and can be 1.5%, 2.5%, 5%, 10%, 20%, 40%, 60%, 80%.

[0040] After obtaining the mixed dispersion, the present invention pours the mixed dispersion onto a nylon filter membrane soaked with metal ions, and after drying, obtains a polyamic acid nanocomposite membrane on the surface of the nylon filter membrane. The present invention has no special requirements for the nylon filter membrane, and a nylon filter membrane well known to those skilled in the art can be used. In the present invention, the surface of the nylon filter membrane is smooth, which is conducive to preparing a smooth and flat membrane. In an embodiment of the present invention, the pore size of the nylon filter membrane is 0.22 μm. 。

[0041] In the present invention, the metal ions preferably include one or more of monovalent metal ions, divalent metal ions and trivalent metal ions, the monovalent metal ions preferably include sodium ions and / or potassium ions, the divalent metal ions preferably include one or more of calcium ions, magnesium ions and copper ions, and the trivalent metal ions preferably include iron ions.

[0042] In the present invention, the nylon filter membrane impregnated with metal ions is preferably obtained by dripping the solution of the metal ions onto the nylon filter membrane, and the nylon filter membrane is preferably placed on a glass plate. In the present invention, the concentration of the metal ions in the solution of the metal ions is preferably 0.1 to 0.5 mol / L, and can be 0.1, 0.2, 0.3, 0.4, or 0.5 mol / L. In the present invention, the solution of the metal ions is preferably an organic solution of the metal ions, specifically obtained by mixing a salt containing the above-mentioned metal ions with an organic solvent, and the organic solvent is preferably N-methylpyrrolidone (NMP). In the present invention, the amount of the solution of the metal ions added is sufficient to ensure that the nylon filter membrane is wetted. In an embodiment of the present invention, the amount of the solution of the metal ions added is 0.8 to 1.0 mL.

[0043] In the present invention, the pouring amount of the mixed dispersion is based on the metal ions infiltrated in the nylon filter membrane being able to fix it (i.e., cross-link it), so that the mixed dispersion does not flow around; in an embodiment of the present invention, the pouring amount of the mixed dispersion is 4 to 6 mL. The present invention pours the mixed dispersion onto the nylon filter membrane infiltrated with metal ions. The shear force generated by the liquid flow during the spreading process of the mixed dispersion induces the nanosheets (nanofillers) to be oriented. The cross-linking of the nanosheets by the metal ions will promptly fix the oriented nanosheets, and a wet film is obtained on the surface of the nylon filter membrane.

[0044] In the present invention, drying is performed immediately after the pouring is completed. In the present invention, the drying preferably includes first drying and second drying in sequence. In the present invention, the temperature of the first drying is preferably 80-120°C, more preferably 100-120°C, and the insulation time is preferably 20-40min, more preferably 30-40min; part of the solvent is volatilized by the first drying. After the first drying, the obtained film is peeled off from the nylon filter membrane. In the present invention, the temperature of the second drying is preferably 200-230°C, more preferably 220-230°C, and the insulation time is preferably 20-40min, more preferably 30-40min; the present invention preferably performs the second drying on the film peeled off from the nylon filter membrane under the condition of fixing all around to prevent the film from curling during the drying process, thereby obtaining a flat film. The present invention removes the remaining solvent by the second drying.

[0045] After obtaining the polyamic acid nanocomposite film, the present invention performs thermal imidization on the polyamic acid nanocomposite film to obtain a polyimide nanocomposite film.

[0046] In the present invention, the thermal imidization preferably includes a first stage and a second stage in sequence, the temperature of the first stage is preferably 300-330°C, more preferably 320-330°C, the holding time is preferably 20-40min, more preferably 30-40min, the temperature of the second stage is preferably 400-430°C, more preferably 410-430°C, the holding time is preferably 90-120min, more preferably 110-120min. In the present invention, the thermal imidization is preferably carried out under a nitrogen atmosphere. After the thermal imidization, the polyamic acid is cyclized to generate polyimide, and the polyimide nanocomposite film is finally obtained.

[0047] The present invention provides a polyimide nanocomposite film prepared by the preparation method described in the above technical solution, wherein the polyimide nanocomposite film comprises a polyimide film and a nanofiller doped in the polyimide film, wherein the nanofiller is cross-linked by metal ions. In the present invention, the doping amount of the nanofiller in the polyimide nanocomposite film is 0-80% (and not 0), and can be 1.5%, 2.5%, 5%, 10%, 20%, 40%, 60%, 80%. The polyimide nanocomposite film provided by the present invention has a high content of nanofillers (up to 80%), is uniform, and has good orientation. The oriented nanofillers can improve the mechanical properties of the composite film, and effectively construct a heat conduction path, improve the thermal conductivity of the composite film, and make the composite film have both high mechanical properties and high thermal conductivity.

[0048] In order to further illustrate the present invention, the polyimide nanocomposite film and the preparation method thereof provided by the present invention are described in detail below in conjunction with examples, but they should not be construed as limiting the protection scope of the present invention.

[0049] In the examples, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2-(4-aminophenyl)-5-aminobenzimidazole (BIA) and N-methylpyrrolidone (NMP) were purchased from Inotech; NMP dispersion of graphene oxide (GO) was purchased from Gaoxin Technology (concentration of 10 mg / mL) and diluted to 3 mg / mL for use. The lateral size of graphene oxide was 3 to 5 μm.

[0050] Example 1

[0051] In this embodiment, a polyimide nanocomposite membrane (GO / PI nanocomposite membrane) is prepared by calcium ion crosslinking, and the steps are as follows:

[0052] (1) Synthesis of PI precursor PAA: First, under a nitrogen atmosphere, 2 mmol of 2-(4-aminophenyl)-5-aminobenzimidazole (BIA) was dissolved in 30 mL of N-methylpyrrolidone (NMP), and then an equal molar amount of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) was added. NMP was then added to make the solid content 10 wt%. After stirring at room temperature for 4 h, a PAA solution was obtained.

[0053] (2) Preparation of polyimide nanocomposite film, the steps are as follows:

[0054] (2.1) mixing the PAA solution obtained in step (1) with a GO NMP dispersion to obtain a mixed dispersion, wherein the mass fraction of GO in the total solids is 2.5%;

[0055] (2.2) Place a nylon filter membrane (pore size of 0.22 μm) on a glass plate, and drip 1 mL of a calcium chloride NMP solution (calcium ion concentration of 0.1 mol / L) onto the filter membrane to wet it; then pour 5 mL of the mixed dispersion obtained in step (2.1) onto the filter membrane. The shear force will induce the nanosheets to orient, and the ionic crosslinking will promptly fix the oriented nanosheets. Then, dry at 120° C. for 40 min to evaporate part of the solvent, and peel the film off the filter membrane;

[0056] (2.3) The film peeled off from the filter membrane was fixed on all sides (to prevent it from curling during the drying process to obtain a flat film), and dried at 230°C for 40 min to remove the remaining solvent to obtain a polyamic acid nanocomposite film, which was recorded as 2.5GO / PAA composite film;

[0057] (2.4) The 2.5GO / PAA composite membrane obtained in step (2.3) was heated at 330°C for 40 min and then at 430°C for 120 min under nitrogen protection to cyclize PAA to generate PI, thereby finally obtaining a polyimide nanocomposite membrane, which was recorded as 2.5GO / PI composite membrane.

[0058] Example 2

[0059] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 1.5%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 1.5GO / PI composite film.

[0060] Example 3

[0061] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 5%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 5GO / PI composite film.

[0062] Example 4

[0063] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 10%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 10GO / PI composite film.

[0064] Example 5

[0065] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 20%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 20GO / PI composite film.

[0066] Example 6

[0067] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 40%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 40GO / PI composite film.

[0068] Example 7

[0069] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 60%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 60GO / PI composite film.

[0070] Example 8

[0071] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 80%, and the rest was the same as Example 1. The obtained polyimide nanocomposite film was recorded as 80GO / PI composite film.

[0072] Example 9

[0073] The dianhydride in step (1) of Example 1 was replaced by pyromellitic dianhydride (PMDA), the diamine was replaced by 4,4'-diaminodiphenyl ether (ODA), and the mass fraction of GO in the total solid in step (2.1) was 0%, 1.5%, 2.5%, 5%, 10%, 20%, 40%, 60%, 80%, respectively, and the rest was the same as Example 1, to obtain polyimide nanocomposite films with different GO contents. The obtained polyimide nanocomposite film is recorded as xGO / PI' (x is the mass fraction of GO) composite film.

[0074] Comparative Example 1

[0075] The mass fraction of GO in the total solid in step (2.1) of Example 1 was adjusted to 0, and the rest was the same as Example 1. A pure polyimide film was obtained, which was recorded as pure PI film.

[0076] Figure 1 The physical pictures of GO / PAA composite films with different GO contents in Example 1, Example 5 and Example 8 are shown in FIG. Figure 1From left to right, the GO / PAA composite films of Example 1, Example 5, and Example 8 correspond to each other. It can be seen that a uniform and smooth film of GO from low concentration to high concentration can be prepared by ionic crosslinking.

[0077] Figure 2 : are the tensile stress-strain curves of the GO / PI composite films with different GO contents prepared in Examples 1 to 8 and Comparative Example 1, Figure 2 Figure a is the tensile stress-strain curve of GO / PI composite films with different GO contents, and figure b is the enlarged view of the first 2% strain in figure a. Figure 2 0, 1.5, 2.5, 5, 10, 20, 40, 60, 80 respectively represent GO / PI composite films with GO contents of 0, 1.5%, 2.5%, 5%, 10%, 20%, 40%, 60%, 80%. Figure 2 The tensile stress-strain curves show that the composite film (2.5GO / PI) containing 2.5wt% GO has extremely high mechanical properties, with a strength of 390MPa, a strain of 33%, and a modulus of 4.1GPa. In comparison, the strength of the pure PI film in Example 1 is 228MPa, the strain is 13%, and the modulus is 3.5GPa. As the GO content increases, the modulus of the composite film continues to increase. The composite film (80GO / PI) containing 80wt% GO has a strength of 70.6MPa, a strain of 0.64%, and a modulus of up to 10.3GPa.

[0078] Figure 3 The in-plane thermal conductivity of the GO / PI composite films with different GO contents prepared in Examples 1 to 8 and Comparative Example 1. It can be seen that the thermal conductivity of the GO / PI composite film also increases significantly with the increase of GO content, and the thermal conductivity of the 80GO / PI composite film can reach 84.8W / (m·K).

[0079] Figure 4 The mechanical properties and thermal conductivity of the PI reported in the industry and laboratory and the GO / PI composite film obtained in the examples of the present invention (Example 1 and Examples 3 to 8, this work) are compared. Figure 4 The left picture in the middle shows the performance comparison of strength and thermal conductivity, and the right picture shows the performance comparison of modulus and thermal conductivity. Figure 4 The corresponding PI types, literature sources and corresponding mechanical properties and thermal conductivity data are listed in Table 1.

[0080] Table 1 PI types, literature sources and corresponding mechanical properties and thermal conductivity data

[0081]

[0082]

[0083] Note: The literature sources represented by the numbers in Table 1 are as follows:

[0084] 1. Ruan, K. et al., Electric-field-induced alignment of functionalized carbon nanotubes inside thermally conductive liquid crystalline polyimide composite films. Angew. Chem. Int. Ed. 62, e202309010 (2023).

[0085] 2. Ruan, K. & Gu, J. Ordered alignment of liquid crystalline graphene fluoride for significantly enhancing thermal conductivities of liquid crystalline polyimide composite films. Macromol. 55, 4134 - 4145 (2022).

[0086] 3. Ma, L., Wang, Y., Xu, X., Wang, Y. & Wang, C. Structural evolution and thermal conductivity of flexible graphite films prepared by carboxylic graphene / polyimide. Ceram. Int. 47, 1076 - 1085 (2021).

[0087] 4. Qu, X., Chen, S., Lu, X. & Lu, Q. Enhancement of thermal conductivity and dimensional stability of polyimide / boron nitride films through mechanochemistry. Compos. Commun. 23, 100549 (2021).

[0088] 5.Qu,X.,Lu,X.Chen,S.&Lu,Q.Thermal conductive hybridpolyimide withultrahigh heat resistance,excellent mechanical properties and low coefficientofthermal expansion.Eur.Polym.J.122,109368(2020).

[0089] 6.Peng,Z.,Guo,Q.,Zhang,L.&Li,C.High thermal conductivity and lowdielectric polyimide nanocomposites using diamine-assisted mechanochemicalexfoliation boron nitride and in-situpolymerizationunderpressure.Chem.Eng.J.488,150824(2024).

[0090] 7.Li,C.et al.,High performances of polyimide / boron nitride nanosheetscomposites via integrativeinterfacialdecorationstrategy.Compos.Sci.Technol.229,109681(2022).

[0091] 8.An,L.etal.,Flexible andquasi-isotropically thermoconductivepolyimide filmsby guided assemblyofboronnitridenanoplate / boronnitrideflakesformicroelectronicapplication.Chem.Eng.J.431,133740(2022).

[0092] 9. Wu, Z. et al., Polyimide-based composites reinforced by carbonnanotube-grafted carbon fiber for improved thermal conductivity and mechanical property. Compos. Commun. 39, 101543 (2023).

[0093] 10.Yu,H.etal.,Thermally conductive,self-healing,andelastic Polyimide@Vertically aligned carbonnanotubes composite as smartthermalinterfacematerial.Carbon 179,348-357(2021).

[0094] 11. Wan, B., Li, X. Zeng,

[0095] 12. Wang,

[0096] By summarizing and comparing the mechanical properties and thermal conductivity of PI reported in industry and laboratories, it can be concluded that the GO / PI nanocomposite film obtained by the ionic crosslinking method of the present invention has extremely high mechanical properties and thermal conductivity.

[0097] Figure 5The scanning electron microscope (SEM) images of GO / PI composite films with different GO contents prepared in Example 1, Examples 3 to 8 and Comparative Example 1. From the SEM images, it can be seen that after adding GO, the composite film has an obvious brick-and-mud structure, and the nanosheets are neatly arranged. Such oriented nanosheets can improve the mechanical properties of the composite film, and effectively construct a heat conduction path to improve the thermal conductivity of the composite film.

[0098] Figure 6 2D WAXS images of GO / PI composite films with different GO contents prepared in Example 1, Examples 2 to 6, Example 8 and Comparative Example 1. Through wide-angle X-ray diffraction (WAXS), it can be concluded that the added nanosheets have a good orientation degree, and the orientation degree of GO in 80GO / PI reaches 0.72, which is the main reason for its excellent mechanical properties and thermal conductivity.

[0099] Figure 7 The SEM images of the xGO / PI' composite membranes with different GO contents prepared in Example 9. From the SEM images, it can be seen that after using PI with different structures, the composite membrane still has an obvious brick-and-mud structure, and the nanosheets are neatly arranged. This oriented arrangement of nanosheets can improve the mechanical properties of the composite membrane, and effectively construct a heat conduction path to improve the thermal conductivity of the composite membrane.

[0100] Figure 8 The in-plane thermal conductivity of the xGO / PI' composite films with different GO contents prepared in Example 9. It can be seen that the thermal conductivity of the films with different PI structures prepared by this method is also significantly improved, which proves the universality of this method.

[0101] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a polyimide nanocomposite film, characterized in that: The following steps are involved: The polyamic acid solution is mixed with a nanofiller to obtain a mixed dispersion; the nanofiller is a nanosheet filler having oxygen-containing groups on the surface; The mixed dispersion is poured onto a nylon filter membrane soaked with metal ions, and after drying, a polyamic acid nanocomposite membrane is obtained on the surface of the nylon filter membrane; The polyamic acid nanocomposite film is thermally imidized to obtain a polyimide nanocomposite film.

2. The preparation method according to claim 1, characterized in that: The solid content of the polyamic acid solution is 10-20 wt %.

3. The preparation method according to claim 1, characterized in that: The nanofiller includes graphene oxide.

4. The preparation method according to claim 1, 2 or 3, characterized in that: The mass of the nanofiller in the mixed dispersion is 0 to 80% of the total solid mass in the mixed dispersion, and is not 0.

5. The preparation method according to claim 1, characterized in that: The metal ions include one or more of monovalent metal ions, divalent metal ions and trivalent metal ions.

6. The preparation method according to claim 5, characterized in that: The monovalent metal ions include sodium ions and / or potassium ions, the divalent metal ions include one or more of calcium ions, magnesium ions and copper ions, and the trivalent metal ions include iron ions.

7. The preparation method according to claim 1, 5 or 6, characterized in that: The nylon filter membrane impregnated with metal ions is obtained by dripping a solution of the metal ions onto the nylon filter membrane, and the concentration of the metal ions in the solution of the metal ions is 0.1-0.5 mol / L.

8. The preparation method according to claim 1, characterized in that: The drying comprises first drying and second drying in sequence, wherein the first drying is carried out at a temperature of 80 to 120° C. and a heat preservation time of 20 to 40 minutes, and the second drying is carried out at a temperature of 200 to 230° C. and a heat preservation time of 20 to 40 minutes; after the first drying, the obtained film is peeled off from the nylon filter membrane.

9. The preparation method according to claim 1, characterized in that: The thermal imidization comprises a first stage and a second stage, wherein the temperature of the first stage is 300-330° C. and the insulation time is 20-40 min, and the temperature of the second stage is 400-430° C. and the insulation time is 90-120 min.

10. A polyimide nanocomposite film prepared by the preparation method according to any one of claims 1 to 9, wherein the polyimide nanocomposite film comprises a polyimide film and nanofillers doped in the polyimide film, wherein the nanofillers are cross-linked by metal ions.