High-safety flame-retardant lithium ion battery electrolyte with low-reactivity coordination structure
By adopting a high-safe flame-retardant electrolyte with a low reactive coordination structure in lithium-ion batteries, and using high-thermal stability salts and low-active solvents to build a weak solvated structure, the lithium-ion battery in traditional electrolytes is easily prone to thermal runaway. Problem, significantly improving the thermal safety and stability of the battery.
Patent Information
- Application Number
- CN202411598944.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-11
- Publication Date
- 2025-02-18
- Estimated Expiration
- 2044-11-11
AI Technical Summary
High-specific energy lithium-ion batteries are prone to thermal runaway, combustion or even explosion in traditional electrolytes. The existing electrolytes produce reducing gas and a large amount of heat in the reaction between the negative electrode and the electrolyte, resulting in thermal runaway.
Using high safety flame retardant lithium-ion battery electrolyte with low reactive coordination structure, using high thermal stability salts such as lithium difluorosulfonimide (LiFSI) as lithium salts, and low-active ester solvents such as dimethyl carbonate (DMC) ) is the main solvent, and ether solvents with weak solvation ability such as 1,1,2,2-tetrafluoroethyl-2,2,3,3 tetrafluoropropyl ether (TTE) are used as sub-solvent, and fluorine is added Additives such as vinyl carbonate are constructed to build a weak solvated structure to improve the stability of the electrolyte.
It effectively slows down the occurrence of side reactions between the electrolyte and the negative electrode, improves the thermal stability on the negative electrode side, improves the thermal safety of lithium-ion batteries, and reduces the danger of combustion and explosion after thermal runaway.
Smart Images

Figure CN119481296A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy storage batteries, and in particular to a highly safe flame-retardant lithium ion battery electrolyte with a low-reactivity coordination structure. Background Art
[0002] Lithium-ion batteries are widely used in portable devices, electric vehicles, and energy storage stations due to their high energy density, long cycle life, and environmental friendliness. However, the thermal safety of high-energy-density lithium-ion batteries poses a huge challenge to their further application. Thermal runaway events caused by the failure of internal materials in lithium-ion batteries are the core cause of thermal safety of lithium-ion batteries. High-energy-density lithium-ion batteries using traditional electrolytes are prone to thermal runaway, combustion, and even explosion.
[0003] The electrolyte plays a key role in ion transfer and has a significant impact on the cost, specific energy, safety, cycle performance, and rate performance of lithium-ion batteries. The electrolyte currently used is composed of lithium salts and organic solvents. The traditional lithium hexafluorophosphate (LiPF6) / ethylene carbonate (EC)-based electrolyte is not suitable for high-specific energy power batteries. During thermal runaway, the reaction between the negative electrode and the electrolyte leads to initial heat accumulation. The EC solvent will first be reduced by the negative electrode to generate reducing gases such as H2, C2H4, and CH4, which are highly explosive. At the same time, LiPF6 will release a large amount of heat after decomposition. In addition, after the positive electrode material phase changes and releases a large amount of oxygen, EC will be oxidized by the oxygen released by the positive electrode, releasing a large amount of heat. This reaction is the thermal runaway triggering reaction in high-nickel batteries.
[0004] In the entire thermal runaway process, the electrolyte plays an indispensable role and becomes the fuse of thermal runaway of lithium-ion batteries. The solvation structure of the traditional electrolyte, which is mainly coordinated by solvent molecules in the first shell, will preferentially decompose on the negative electrode surface. Compared with solvent coordination, the solvation structure in which anions participate in coordination significantly increases the energy of the lowest unoccupied molecular orbital (LUMO), which indicates that anion coordination enhances the reduction stability of the electrolyte.
[0005] Therefore, rational design of the coordination and concentration of the electrolyte can suppress the exothermic reaction between the highly reactive negative electrode and the electrolyte, thereby improving the safety of high-energy-density lithium-ion batteries. Summary of the invention
[0006] The present invention aims to solve the technical problems existing in the traditional electrolyte of the high-energy-density lithium-ion battery mentioned above and provide a high-safety flame-retardant lithium-ion battery electrolyte with a low-reactivity coordination structure, aiming to improve the thermal safety performance of the high-energy-density lithium-ion battery.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0008] The present invention first provides a high-safety flame-retardant lithium-ion battery electrolyte with a low-reactivity coordination structure. The low-reactivity high-safety flame-retardant electrolyte uses a high thermal stability salt as a lithium salt, a low-activity ester solvent as a main solvent, an ether solvent with weak solvation ability as a secondary solvent, and additives.
[0009] Furthermore, the high thermal stability lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI). Since the decomposition temperature of LiFSI is above 300°C, while the decomposition temperature of the traditional lithium salt LiPF6 is around 100°C, adding LiFSI can improve the stability of the electrolyte.
[0010] Furthermore, the low-activity ester solvent is selected from one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), or a mixture of the above-mentioned solvents in any proportion.
[0011] Furthermore, the ether solvent with weak solvating ability is one or more of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE) with higher lowest unoccupied molecular orbital (LUMO) energy value. The above ether solvents can well block electron transmission and have strong anti-reduction ability.
[0012] Furthermore, the additive is selected from one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC) and lithium hexafluorophosphate (LiPF6).
[0013] Furthermore, the concentration of the lithium salt in the low-reactivity high-safety flame-retardant electrolyte is 1.0-2.0 mol / L, and the volume ratio of the ester solvent to the ether solvent in the electrolyte is (3-6): (4-7). Since the ether solvent hardly participates in the solvation structure and has more of a dilution effect, the use of this concentration ratio can not only ensure the advantages of the contact ion pair and ion aggregate structure, that is, construct an anion-derived interface and improve the interface stability), but also avoid the disadvantages of high viscosity and slow ion transmission. Among the additives, if the fluoroethylene carbonate is added, its mass accounts for 2%-10% of the low-reactivity high-safety flame-retardant electrolyte; if the vinylene carbonate additive is added, its mass accounts for 2%-10% of the total mass of the high-safety low-reactivity electrolyte; if the lithium hexafluorophosphate is added, its mass accounts for 1%-2% of the total mass of the high-safety low-reactivity electrolyte.
[0014] Furthermore, compared with the cyclic coordination structure of the traditional electrolyte, the low-reactivity chain coordination structure has a higher lowest unoccupied molecular orbital (LUMO), a stronger ability to block electron transmission, and a stronger ability to resist reduction. Since the EC solvent in the traditional electrolyte is cyclic, the cyclic unsaturated bond is easy to break. Compared with the traditional electrolyte Li + -The cyclic unsaturated bond in the EC coordination structure and the low-reactivity coordination structure in the present invention are less likely to break the bond and produce reducing gases such as C2H4 and H2.
[0015] Furthermore, the preparation method of the electrolyte of the present invention is: in an argon-protected glove box, first weigh the lithium salt, then add the main solvent, the secondary solvent and the additive in proportion, and stir evenly to form a mixed solution, so as to obtain the high-safety flame-retardant lithium-ion battery electrolyte with a low-reactivity coordination structure.
[0016] Furthermore, the ion coordination number ratio of lithium ions, anions, and main solvent in the weak solvation structure is 1:(2-3):(2-3). The meaning of the ion coordination number is: the ratio of the number of lithium ions to the number of molecules of the main solvent and the secondary solvent in the electrolyte solvation structure. This ratio can help form anion-rich (FSI) - ) interface, which is more stable and can improve battery safety.
[0017] The present invention also provides a lithium ion battery, comprising a positive electrode active material, a negative electrode active material, an electrolyte and a separator, wherein the electrolyte is the above-mentioned low-reactivity high-safety flame-retardant electrolyte.
[0018] Furthermore, the positive electrode active material is LiNi x Co y Mn z O2, where x ≥ 0.8, 0.1 ≥ y ≥ 0.05, 0.1 ≥ z ≥ 0.05.
[0019] Furthermore, the negative electrode active material is selected from one or more of natural graphite, artificial graphite, and silicon-carbon composite materials.
[0020] Furthermore, the diaphragm is selected from any one of polypropylene film PP, polyethylene film PE, and PP / PE composite film.
[0021] Furthermore, the battery energy density is ≥250Wh kg -1 .
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] The electrolyte in the present invention constructs a weak solvation structure. Through theoretical calculations, compared with traditional electrolytes, the high-safety and low-reactivity electrolyte has a higher lowest unoccupied molecular orbital (LUMO), lower electrophilicity and anti-reduction ability, thereby effectively slowing down the side reactions between the electrolyte and the negative electrode and improving the thermal stability of the negative electrode side.
[0024] The electrolyte of the present invention uses lithium salts with higher thermal stability and inert solvents with low reactivity to replace the highly reactive substances in traditional electrolytes, which can effectively improve the thermal safety of single cells. Specifically, it is manifested in higher thermal failure starting temperature and trigger temperature during thermal runaway, and lower maximum thermal runaway temperature.
[0025] The electrolyte of the present invention adopts one or more of the flame retardant solvents 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE), which can effectively inhibit the generation of reducing gas in high-energy lithium-ion batteries and further reduce the combustion and explosion hazards after thermal runaway of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 is the lowest unoccupied molecular orbital diagram of different electrolyte components;
[0028] Figure 2 It is adiabatic thermal runaway curve diagram corresponding to Example 1 and Comparative Example 1;
[0029] Figure 3 The heat flow curves of thermal failure of materials corresponding to Example 1 and Comparative Example 1;
[0030] Figure 4 It is a curve diagram of thermal failure reducing gas of materials corresponding to Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0031] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0032] Example 1
[0033] This embodiment provides a high-safety, low-reactivity lithium-ion battery electrolyte based on a local weak solvation of an ester solvent as the main solvent, which is as follows:
[0034] The positive electrode active material of lithium-ion battery is LiNi 0.9 Co 0.05 Mn 0.05 O2, the negative electrode active material is silicon carbon (90% Gr@10% SiO), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0035] Preparation of electrolyte: The raw material composition includes lithium salt, ester main solvent, ether secondary solvent and additive. The volume fraction of ester main solvent and ether secondary solvent is: dimethyl carbonate: 1,1,2,2-tetrafluoroethyl-2,2,3,3 tetrafluoropropyl ether = 3:7. The lithium salt is lithium bis(fluorosulfonyl)imide, and the concentration in the electrolyte is 1.2 mol / L. The electrolyte additive is vinylene carbonate, and its mass accounts for 4% of the total mass of the electrolyte. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and the ether solvent are added in sequence according to the proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, that is, a high-safety, low-reactivity electrolyte with local weak solvation for high-energy lithium-ion batteries is obtained.
[0036] Example 2
[0037] This embodiment provides a high-safety, low-reactivity lithium-ion battery electrolyte based on a local weak solvation of an ester solvent as the main solvent, which is as follows:
[0038] The positive electrode active material of lithium-ion battery is LiNi 0.9 Co 0.05 Mn 0.05 O2, the negative electrode active material is graphite (Gr), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0039] Preparation of electrolyte: The raw materials include lithium salt, ester main solvent, ether secondary solvent and additive. The volume fraction of ester main solvent and ether secondary solvent is: dimethyl carbonate: 1,1,2,2-tetrafluoroethyl-2,2,3,3 tetrafluoropropyl ether = 4:6. The lithium salt is lithium bis(fluorosulfonyl)imide, and the concentration in the electrolyte is 1.5 mol / L. The electrolyte additives are vinylene carbonate and fluoroethylene carbonate, and their mass proportions are 2% and 3% of the total mass of the electrolyte, respectively. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and ether solvent are added in sequence according to the proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, that is, a high-safety, low-reactivity electrolyte with local weak solvation for high-energy lithium-ion batteries is obtained.
[0040] Example 3
[0041] This embodiment provides a high-safety, low-reactivity lithium-ion battery electrolyte based on a local weak solvation of an ester solvent as the main solvent, which is as follows:
[0042] The positive electrode active material of lithium-ion battery is LiNi 0.8 Co 0.1 Mn 0.1 O2, the negative electrode active material is graphite (Gr), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0043] Preparation of electrolyte: The raw material composition includes lithium salt, ester main solvent, ether secondary solvent and additive. The volume fraction of ester main solvent and ether secondary solvent is: dimethyl carbonate: 1,1,2,2-tetrafluoroethyl-2,2,3,3 tetrafluoropropyl ether = 6:4. The lithium salt is lithium bis(fluorosulfonyl)imide, and the concentration in the electrolyte is 1.1 mol / L. The electrolyte additive is lithium hexafluorophosphate, and its mass accounts for 2% of the total mass of the electrolyte. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and ether solvent are added in sequence according to the proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, that is, a high-safety, low-reactivity electrolyte with local weak solvation for high-energy lithium-ion batteries is obtained.
[0044] Example 4
[0045] This embodiment provides a high-safety, low-reactivity lithium-ion battery electrolyte based on a local weak solvation of an ester solvent as the main solvent, which is as follows:
[0046] The positive electrode active material of lithium-ion battery is LiNi 0.8 Co 0.1 Mn 0.1 O2, the negative electrode active material is silicon carbon (Gr), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0047] Preparation of electrolyte: The raw material composition includes lithium salt, ester main solvent, ether secondary solvent and additive. The volume fraction of ester main solvent and ether secondary solvent is: dimethyl carbonate: 1,1,2,2-tetrafluoroethyl-2,2,3,3 tetrafluoropropyl ether: 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE) = 3:4:3. The lithium salt is lithium bis(fluorosulfonyl)imide, and the concentration in the electrolyte is 1.2 mol / L. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and ether solvent are added in proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, that is, a high-safety, low-reactivity electrolyte with local weak solvation for high-energy lithium-ion batteries is obtained.
[0048] Comparative Example 1
[0049] This comparative example provides a traditional electrolyte based on an ester solvent as the main solvent, which is as follows:
[0050] The positive electrode active material of lithium-ion batteries is LiNi 0.9 Co 0.05 Mn 0.05 O2, the negative electrode active material is graphite (Gr), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0051] Preparation of electrolyte: The raw materials include lithium salt, ester solvent and additive. The volume fraction of ester solvent is: ethylene carbonate: ethyl methyl carbonate = 3:7. The lithium salt is lithium hexafluorophosphate, and the concentration in the electrolyte is 1 mol / L. The additive is fluoroethylene carbonate, and its mass accounts for 1% of the total mass of the electrolyte. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and ether solvent are added in proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, so as to obtain a high-energy lithium-ion battery with a high safety and low reactivity electrolyte with local weak solvation.
[0052] Comparative Example 2
[0053] This comparative example provides a traditional electrolyte based on an ester solvent as the main solvent, which is as follows:
[0054] The positive electrode active material of lithium-ion batteries is LiNi 0.9 Co 0.05 Mn 0.05 O2, the negative electrode active material is silicon carbon (90% Gr@10% SiO), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0055] Preparation of electrolyte: The raw materials include lithium salt, ester solvent and additive. The volume fraction of ester solvent is: ethylene carbonate: ethyl methyl carbonate = 3:7. The lithium salt is lithium hexafluorophosphate, and the concentration in the electrolyte is 1 mol / L. The additive is fluoroethylene carbonate, and its mass accounts for 1% of the total mass of the electrolyte. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and ether solvent are added in proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, so as to obtain a high-energy lithium-ion battery with a high safety and low reactivity electrolyte with local weak solvation.
[0056] Comparative Example 3
[0057] This comparative example provides a traditional electrolyte based on an ester solvent as the main solvent, which is as follows:
[0058] The positive electrode active material of lithium-ion batteries is LiNi 0.8 Co 0.1 Mn 0.1 O2, the negative electrode active material is graphite (Gr), and the diaphragm is PP diaphragm with ceramic single-sided coating.
[0059] Preparation of electrolyte: The raw materials include lithium salt, ester solvent and additive. The volume fraction of ester solvent is: ethylene carbonate: ethyl methyl carbonate = 3:7. The lithium salt is lithium hexafluorophosphate, and the concentration in the electrolyte is 1 mol / L. The additive is fluoroethylene carbonate, and its mass accounts for 1% of the total mass of the electrolyte. The preparation of the electrolyte is carried out in an argon-protected glove box (H2O≤0.1ppm, O2≤0.1ppm). During the preparation, the lithium salt is weighed first, and then the ester solvent and ether solvent are added in proportion, and then the additive is added, and the mixture is stirred evenly to form a mixed solution, so as to obtain a high-energy lithium-ion battery with a high safety and low reactivity electrolyte with local weak solvation.
[0060] The thermal runaway characteristic temperature of the single battery and the material thermal failure starting temperature and heat flow of the above-mentioned Examples 1-4 and Comparative Examples 1-3 are as follows:
[0061] 1. Battery charge and discharge test conditions: constant current and constant voltage charging and constant current discharge, the voltage range is 2.8-4.2V. Examples 1-4 and Comparative Examples 1-3 were charged to 4.2V at 30°C, respectively, the battery reached 100% SOC in the fully charged state, and the safety performance was tested. The test conditions for the single cell thermal runaway experiment are: an adiabatic calorimeter is used to measure the thermal safety of the fully charged single cell, the starting heating temperature is 50°C, the ending heating temperature is 300°C, the temperature step is 10°C, and the waiting time is 25min. The starting exothermic temperature T1 of thermal runaway self-generation is defined as the temperature rise rate greater than 0.02°C min -1 The thermal runaway trigger temperature T2 is defined as the temperature rise rate greater than 1°C s -1 The thermal stability test conditions of battery materials are as follows: the thermal stability of fully charged battery materials is tested using a differential scanning calorimeter, the heating temperature range is 50-550°C, and the temperature rise rate is 10°C min -1 The measured thermal runaway characteristic temperature of the single cell, the thermal failure starting temperature of the material and the heat flow are shown in Table 1:
[0062] Table 1
[0063]
[0064] As shown in Table 1, under the adiabatic thermal runaway test conditions, the thermal runaway self-heating starting temperature of the fully charged battery assembled with the electrolyte of Example 1 is 152.9°C, the thermal runaway triggering temperature is 260.2°C, and the thermal runaway maximum temperature is 809.2°C. Compared with Comparative Example 1, the thermal runaway starting temperature is increased by 38°C, the triggering temperature is increased by 77°C, and the maximum temperature is reduced by 284°C. The thermal failure test results of the full-charge battery material positive electrode + negative electrode + electrolyte show that the thermal failure starting temperature of the material in Example 1 is 102.4°C, which is 19°C higher than that in Comparative Example 1, and the heat flow rate of Example 1 is 786 J g -1 , which is 510 J g lower than that of comparative example 1 -1 This indicates that the highly safe flame-retardant electrolyte with low-reactivity coordination can effectively delay the failure temperature of battery materials, inhibit interfacial side reactions to further reduce heat release, and effectively improve the safety performance of the battery.
[0065] Figure 1 The lowest unoccupied molecular orbital diagram of the electrolyte components used in Examples 1-3 and Comparative Examples 1-3 of the present invention. By comparison, it can be seen that the LUMO energy of the electrolyte solvent component in the embodiment is higher than the solvent EC in the comparative example, and the LUMO energy of the electrolyte solvation structure in Example 1 is also higher than the LUMO energy of the solvation structure in Comparative Example 4, indicating that the electrolyte in the embodiment has lower electrophilicity and higher anti-reduction ability, which can effectively slow down the exothermic side reaction between the electrolyte and the negative electrode, and improve the thermal stability of the negative electrode side.
[0066] Figure 2 The adiabatic thermal runaway curves for Example 1 and Comparative Example 2 are shown in FIG. As can be seen from the figure, the battery in Example 1 also has a higher self-heating starting temperature and thermal runaway trigger temperature, as well as a lower thermal runaway maximum temperature during thermal runaway. The thermal runaway starting temperature increased by 38°C, the trigger temperature increased by 77°C, and the maximum temperature decreased by 284°C, indicating that the thermal safety performance of the battery obtained in Example 1 is effectively improved.
[0067] Figure 3 The heat flow curves of thermal failure of materials corresponding to Example 1 and Comparative Example 1 are shown. The thermal failure starting temperature of the material in Example 1 is 102.4°C, which is 19°C higher than that in Comparative Example 1. The heat flow of Example 1 is 786 J g -1 , which is 510 J g lower than that of comparative example 1 -1 This indicates that the electrolyte in Example 1 can effectively delay the failure temperature of battery materials, inhibit interface side reactions, further reduce heat release, and improve the safety performance of the battery.
[0068] Figure 4The graphs of thermal failure reducing gas of materials corresponding to Example 1 and Comparative Example 1 show that the proportion of reducing gas after thermal runaway of the battery in Example 1 is much smaller than that of the battery in Comparative Example 1, indicating that the electrolyte in Example 1 has a coordination structure with lower reactivity, and the chain CO bond breaking ability in the coordination structure is weaker than that of the conventional Li in Comparative Example 1. + -EC's ability to break CO bonds in the cyclic chain can effectively reduce the generation of reducing gases such as C2H4 and H2.
[0069] From the above, it can be seen that the present invention provides a high-safety flame-retardant electrolyte with low-reactivity coordination, with a high thermal stability salt as a lithium salt, a low-activity ester solvent as a main solvent, an ether solvent with weak solvation ability as a secondary solvent and an inert diluent, and additives are added, so that the lithium-ion battery prepared by it has good thermal safety performance. The selected solvent combines the advantages of multiple solvents: high LUMO energy level, good anti-reduction performance, can effectively inhibit the redox reaction of the negative electrode side of the battery and the electrolyte, and reduce heat accumulation; the high-safety flame-retardant electrolyte has a low-reactivity coordination structure, which can effectively inhibit the generation of reducing gas and reduce the external combustion hazard of the battery; the selected lithium salt is a high-stability lithium salt with good thermal stability; by optimizing the ratio of solvent and lithium salt, the solvation structure of the electrolyte is effectively improved, and the battery safety is further improved. At the same time, the additives used can assist in the construction of an inorganic-rich electrolyte interface and improve the interface stability.
[0070] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure, characterized in that: The low-reactivity and high-safety flame-retardant electrolyte uses a high-thermal stability salt as a lithium salt, a low-activity ester solvent as a main solvent, an ether solvent with a weak solvating ability as a secondary solvent, and additives.
2. The highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to claim 1, characterized in that: The high thermal stability lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI).
3. The highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to claim 2, characterized in that: The low-activity ester solvent is selected from one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC).
4. The highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to claim 3, characterized in that: The ether solvent with weak solvating ability is selected from one or more of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE).
5. The highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to claim 4, characterized in that: The additive is selected from one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC) and lithium hexafluorophosphate (LiPF6).
6. The highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to any one of claims 1 to 5, characterized in that: The concentration of the lithium salt in the low-reactivity, high-safety, flame-retardant electrolyte is 1.0-2.0 mol / L, and the volume ratio of the ester solvent to the ether solvent in the electrolyte is (3-6):(4-7).
7. The highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to claim 6, characterized in that: Among the additives, if the fluoroethylene carbonate is added, its mass accounts for 2% to 10% of the low-reactivity and high-safety flame-retardant electrolyte; if the vinylene carbonate additive is added, its mass accounts for 2% to 10% of the total mass of the high-safety and low-reactivity electrolyte; if the lithium hexafluorophosphate is added, its mass accounts for 1% to 2% of the total mass of the high-safety and low-reactivity electrolyte.
8. The method for preparing a highly safe flame-retardant lithium-ion battery electrolyte having a low-reactivity coordination structure according to any one of claims 1 to 7, characterized in that: In an argon-protected glove box, lithium salt is first weighed, and then a main solvent, a secondary solvent and an additive are added in order according to a proportion, and stirred evenly to form a mixed solution, thereby obtaining the highly safe flame-retardant lithium-ion battery electrolyte with a low-reactivity coordination structure.
9. A lithium ion battery comprising a positive electrode active material, a negative electrode active material, an electrolyte and a separator, characterized in that: The electrolyte is the electrolyte according to any one of claims 1 to 7.
10. The lithium ion battery according to claim 9, characterized in that: The positive electrode active material is LiNi x Co y Mn z O2, where x ≥ 0.8, 0.1 ≥ y ≥ 0.05, 0.1 ≥ z ≥ 0.05; The negative electrode active material is selected from one or more of natural graphite, artificial graphite, and silicon-carbon composite materials; The diaphragm is selected from any one of polypropylene film PP, polyethylene film PE, and PP / PE composite film; The battery energy density is ≥250Wh kg -1 .
Citation Information
Patent Citations
Ultra-high-temperature safe lithium ion battery electrolytic solution and lithium ion battery using electrolytic solution
CN111564665A
Fluoroether self-flame-retardant electrolyte for disposable lithium battery
CN115632136A
Lithium-ion battery
JP2023159870A
Electrolyte for lithium secondary batteries and lithium secondary battery including the same
US20150249269A1
Cited By
High-safety reduction-resistant solid-liquid composite electrolyte as well as preparation method and application thereof
CN120497453A
Electrolyte based on low-dosage ethylene carbonate and application of electrolyte in secondary battery
CN120978215A