A polyhydroxyazo-grafted graphene oxide-based material and its application in electromagnetic wave absorption.

By introducing benzene azo groups onto the surface of polyhydroxy graphene oxide and covalently grafting it, the impedance mismatch problem of graphene-based materials was solved, achieving high-efficiency electromagnetic wave absorption performance. This method is suitable for lightweight, efficient, and stable electromagnetic microwave absorbing materials.

CN119822363BActive Publication Date: 2025-11-14NANJING UNIV OF INFORMATION SCI & TECH

Patent Information

Application Number
CN202510046616.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-01-13
Publication Date
2025-11-14
Estimated Expiration
2045-01-13

AI Technical Summary

Technical Problem

In the existing technology, the impedance mismatch caused by the high conductivity of pure graphene weakens its electromagnetic wave absorption ability, and there is no mature technology that can effectively improve the electromagnetic wave absorption performance of polyhydroxyl oxide graphene-based materials.

Method used

By introducing benzene azo groups onto the surface of polyhydroxy graphene oxide-based materials and performing covalent grafting modification using the diazo coupling method, impedance matching is coordinated, conductivity is reduced, and electromagnetic waves are absorbed synergistically through mechanisms such as polarization loss, interlayer multiple reflections and scattering.

Benefits of technology

A lightweight, efficient, and stable electromagnetic microwave absorbing material has been developed, which has good microwave absorption performance and is suitable for the development of lightweight, efficient, and stable electromagnetic microwave absorbing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119822363B_ABST
    Figure CN119822363B_ABST
Patent Text Reader

Abstract

This invention provides a benzene-azo group-grafted polyhydroxy graphene oxide-based material and its application in electromagnetic wave absorption. The material is synthesized using aniline compounds and polyhydroxy graphene oxide as raw materials via diazo coupling. The feasibility of the preparation method was verified by spectral characterization, demonstrating the feasibility of impedance matching through covalent grafting of functionalized functional groups. This preparation method is simple, low-cost, and yields high output.
Need to check novelty before this filing date? Find Prior Art

Description

Technical fields:

[0001] This invention relates to a microwave absorbing material, specifically to a polyhydroxy graphene oxide-based material grafted with a benzene azo group and its application in electromagnetic wave absorption. Background technology:

[0002] The rapid development of electronic communication technology has made electromagnetic radiation pollution a globally recognized major environmental problem. Large amounts of electromagnetic radiation not only damage precision electronic equipment but also pose a significant threat to human health. Therefore, developing microwave absorbing materials with characteristics such as lightweight, high microwave absorptivity, thin matching thickness, and wide absorption bandwidth is imperative. Two-dimensional materials, especially graphene, have gradually become one of the most attractive candidate materials due to their excellent chemical and physical properties, such as low density, large specific surface area, high electron mobility, good thermal stability, and corrosion resistance. However, the impedance mismatch caused by the high conductivity of pure graphene weakens its electromagnetic wave absorption capability. Therefore, adjusting conductivity to coordinate impedance is currently a key research direction in the development of efficient graphene-based microwave absorbing materials. Utilizing the tunable dielectric properties of graphene oxide and reduced graphene oxide, functionalization modification can be achieved through chemical reactions with the oxygen-containing functional groups on their surface, thereby improving the aforementioned problems.

[0003] Existing research has demonstrated that covalent modification of functional groups can alter the electronic structure and transport properties of graphene-based materials. Due to their chemical stability and rapid response characteristics, azo compounds hold great potential in enhancing the photoelectric properties of graphene derivatives, contributing to improved electromagnetic wave absorption performance of graphene-based materials. However, currently, there is no mature technology to obtain polyhydroxyl oxide graphene-based materials capable of absorbing electromagnetic waves. Summary of the Invention:

[0004] To address the problems existing in the prior art, this invention provides a polyhydroxy graphene oxide-based material grafted with a benzene azo group and its application in electromagnetic wave absorption.

[0005] The specific technical solution of the present invention is as follows:

[0006] A polyhydroxyl oxide graphene-based material grafted with a benzene azo group, the preparation method of which is as follows:

[0007] Step 1: Add aniline compounds to dilute hydrochloric acid solution, heat until completely dissolved, and then cool under low temperature conditions;

[0008] Step 2: Add sodium nitrite solution dropwise to the solution prepared in Step 1, react fully under low temperature conditions, add urea to remove excess sodium nitrite, stir, and obtain diazonium salt;

[0009] Step 3: Take the polyhydroxy graphene oxide suspension and adjust the pH to 8-10 using alkaline buffer solution;

[0010] Step 4: Add the diazonium salt prepared in step 2 to the suspension prepared in step 3, and continue stirring under low temperature conditions to carry out the coupling reaction;

[0011] Step 5: After the coupling reaction is complete, filter, wash, and vacuum dry to obtain a polyhydroxy graphene oxide-based material grafted with benzene azo groups.

[0012] In the above steps, the molar ratio of aniline compounds, sodium nitrite, and dilute hydrochloric acid is 1:(1.05~1.15):(2.5~5.5); the molar ratio of aniline compounds to polyhydroxy graphene oxide is 200:1.

[0013] A further design of the present invention is that, in step 1, the aniline compound is p-bromoaniline, p-chloroaniline, or p-trifluoromethylaniline.

[0014] A further design feature is that the low-temperature condition is a 0-5°C ice-water bath.

[0015] A further design feature is that, in step 4, the coupling reaction time is 4 to 7 hours.

[0016] A further design feature is that, in step 1, the concentration of the dilute hydrochloric acid is 4–6 mol / L.

[0017] A further design element is that, in step 3, the polyhydroxy graphene oxide suspension is prepared by the following method:

[0018] 1) Graphene oxide was dispersed in DMSO, manganese acetate was added as a catalyst, and the mixture was stirred until a suspension was formed. The pH was then adjusted to 4 with dilute hydrochloric acid solution.

[0019] 2) Irradiate the suspension with ultraviolet light for 8 days, add ZnO and isopropanol, and continue to irradiate with ultraviolet light for 8 days to obtain a polyhydroxy graphene oxide suspension.

[0020] A further design feature is that, in step 3, the alkaline buffer solution is a buffer solution prepared from sodium carbonate and sodium bicarbonate.

[0021] Further design involves adding an appropriate amount of dilute hydrochloric acid after the coupling reaction in step 4, heating and stirring to remove excess alkaline buffer solution until the pH value is 7; then raising the temperature to 50°C and stirring for 4 hours to remove byproducts.

[0022] A further design feature is that, in step 5, the vacuum drying temperature is 80–120°C, and the time is 48 hours.

[0023] Applications of the aforementioned polyhydroxyapatite-grafted polyhydroxyapatite-based materials in microwave absorption.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) This invention uses aniline compounds and polyhydroxy graphene oxide as raw materials to synthesize a polyhydroxy graphene oxide-based microwave absorbing material grafted with phenylazo groups via diazo coupling. The feasibility of the preparation method was verified by spectral characterization, namely, the feasibility of covalently grafting functional groups to coordinate impedance matching. This preparation method is simple, low-cost, and has a high yield.

[0026] (2) Due to their high conductivity, graphene-based materials can lead to impedance mismatch. The microwave absorbing material provided in this invention introduces benzene azo groups on the surface of the graphene-based material. Benzoazo groups are non-conductive groups, and when grafted onto the graphene-based material, they disrupt the original electron transport path of graphene, increase the resistance to electron movement, and thus reduce the conductivity of the material, thereby coordinating impedance matching. At the same time, the steric hindrance effect generated by the introduction of benzene azo groups can reduce electron transport efficiency, effectively restrict the conductive network, and thus optimize impedance matching.

[0027] (3) The polyhydroxyl oxide graphene-based microwave absorbing material grafted with benzene azo groups provided by this invention can dissipate electromagnetic waves through multiple mechanisms such as polarization loss, interlayer multiple reflection and scattering, and conduction loss, exhibiting excellent microwave absorption performance. It provides a feasible technology for developing lightweight, efficient, and stable electromagnetic microwave absorbing materials.

[0028] (4) The present invention rationally selects the coupling reaction time, the molar ratio of aniline compound and dilute hydrochloric acid, and the molar ratio of aniline compound and sodium nitrite, which ensures the product yield and facilitates mass industrial production.

[0029] (5) The present invention reasonably adjusts the pH range of the polyhydroxy graphene oxide suspension to 8-10. When the pH of the suspension is below 8, the phenolic hydroxyl groups cannot form phenoxy anions, and the reaction rate is slow or even cannot proceed; when the pH of the suspension is above 10, the diazonium salt will react with OH- - The reaction occurs, generating diazoic acid or diazoic acid anions, which cause it to lose its coupling ability and reduce the reaction yield. Attached image description:

[0030] Figure 1 This is a schematic diagram of the synthesis route of the polyhydroxyazo group-grafted graphene oxide-based microwave absorbing material prepared in the embodiments of the present invention;

[0031] Figure 2 The image shows the FT-IR spectrum of the polyhydroxyapatite-based microwave absorbing material grafted with benzene azo groups prepared in the embodiments of the present invention.

[0032] Figure 3 The XRD pattern of the polyhydroxyapatite-based microwave absorbing material grafted with benzene azo groups prepared in the embodiments of the present invention is shown below.

[0033] Figure 4 The reflection loss, impedance matching, and frequency correlation spectra of the ring test sample made from the benzene azo group-grafted polyhydroxy oxide graphene-based microwave absorbing material prepared in the embodiments of the present invention are shown. Detailed implementation method:

[0034] The invention will be further described below with reference to examples:

[0035] Preparation of polyhydroxyl graphene oxide suspension:

[0036] Polyhydroxy graphene oxide is a type of graphene oxide, and its preparation process is as follows:

[0037] 1) Disperse graphene oxide (0.4g) in dimethyl sulfoxide (DMSO) (200mL), add manganese acetate as a catalyst, stir evenly to form a suspension, and adjust its pH to 4 with dilute hydrochloric acid solution.

[0038] 2) Irradiate the suspension with ultraviolet light (λ = 185 nm) for 8 days, then add ZnO and isopropanol, and continue irradiation with ultraviolet light (λ = 185 nm) for another 8 days to obtain a polyhydroxy graphene oxide suspension. This was used in the following examples.

[0039] Example 1.

[0040] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0041] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0042] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0043] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0044] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (0.25 g).

[0045] Example 2.

[0046] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (8.25 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0047] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0048] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0049] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0050] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (0.23 g).

[0051] Example 3.

[0052] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (3.75 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0053] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0054] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0055] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0056] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.22g).

[0057] As can be seen from Examples 1-3, when the molar ratio of p-bromoaniline to dilute hydrochloric acid is between 1:2.5 and 5.5, the product mass first increases and then decreases. Therefore, the following examples will be described with a molar ratio of p-bromoaniline to dilute hydrochloric acid of 1:4.

[0058] Example 4.

[0059] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0060] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0061] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0062] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0063] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.23g).

[0064] Example 5.

[0065] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0066] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0067] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0068] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0069] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.25g).

[0070] As shown in Examples 1, 4, and 5, when the molar ratio of p-bromoaniline to sodium nitrite is less than 1:1.05, the diazotization reaction of p-bromoaniline is incomplete, resulting in a decrease in product mass; when the molar ratio is greater than 1:1.15, the product mass remains essentially unchanged, leading to waste of sodium nitrite. Therefore, the following examples will be described with a molar ratio of p-bromoaniline to sodium nitrite of 1:1.1.

[0071] Example 6.

[0072] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (-3 to 0 °C).

[0073] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0074] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0075] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0076] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.22g).

[0077] Example 7.

[0078] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (5-8 °C).

[0079] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0080] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0081] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 4 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0082] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.21g).

[0083] As can be seen from Examples 1, 6, and 7, when the reaction temperature is below 0°C, the diazotization reaction rate is slow and the reaction yield is reduced; when the reaction temperature is above 5°C, the decomposition of the diazonium salt is accelerated, which also reduces the yield.

[0084] Example 8.

[0085] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0086] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0087] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0088] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 2 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0089] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.21g).

[0090] Example 9.

[0091] (1) Add p-bromoaniline (1.03 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-bromoaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0092] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0093] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-bromoaniline to polyhydroxy graphene oxide is 200:1.

[0094] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the coupling reaction was continued for 8 hours with stirring in an ice-water bath. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and stirring was continued for 4 hours to remove byproducts.

[0095] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-bromophenylazo-grafted polyhydroxy graphene oxide (PBPA-MHGO, 0.24g).

[0096] As can be seen from Examples 1, 8, and 9, when the coupling reaction time is less than 4 hours, the coupling reaction is incomplete and the reaction yield is low; when the coupling reaction time is more than 7 hours, the unreacted diazonium salt gradually decomposes, the reaction will not continue, and the yield remains basically unchanged.

[0097] Example 10.

[0098] (1) Add p-chloroaniline (0.77 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mmol / L), heat to completely dissolve p-chloroaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0099] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0100] (3) Add 150 mL of polyhydroxy graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of p-chloroaniline to polyhydroxy graphene oxide is 200:1.

[0101] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the mixture was stirred in an ice-water bath for 4 hours. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and the mixture was stirred for 4 hours to remove byproducts.

[0102] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-chlorophenyl azo-grafted polyhydroxy graphene oxide (PCPA-MHGO, 0.28g).

[0103] Example 11.

[0104] (1) Add p-trifluoromethylaniline (0.97 g, 6 mmol) to a dilute hydrochloric acid solution (6 mL, 4 mol / L), heat to completely dissolve p-trifluoromethylaniline, and then cool the solution in an ice-water bath (0-5 °C).

[0105] (2) Dissolve sodium nitrite (0.46 g, 6.6 mmol) in 4 mL of water to obtain an aqueous solution of sodium nitrite. Slowly add the aqueous solution of sodium nitrite dropwise to the solution obtained in step 1 and stir in an ice-water bath for 30 minutes. Then add urea (10 mg, 0.2 mmol) to remove excess sodium nitrite and continue stirring for 10 minutes to obtain a diazonium salt solution.

[0106] (3) Add 150 mL of polyhydroxyl graphene oxide suspension to a three-necked flask. Dissolve sodium bicarbonate (0.42 g, 5 mmol) and sodium carbonate (0.20 g, 2 mmol) in water (50 mL) to prepare an alkaline buffer solution to adjust the pH of the suspension. Place the flask in an ice-water bath and stir. The molar ratio of trifluoromethylaniline to polyhydroxyl graphene oxide is 200:1.

[0107] (4) The prepared diazonium salt solution was slowly added dropwise to the above suspension, and the mixture was stirred in an ice-water bath for 4 hours. Dilute hydrochloric acid was added to remove excess sodium bicarbonate and sodium carbonate until the pH value was 7. Then the temperature was raised to 50°C and the mixture was stirred for 4 hours to remove byproducts.

[0108] (5) After the reaction was completed, the system was cooled to room temperature, filtered, washed with water, and dried under vacuum at 80°C for 48 hours to obtain the product p-trifluoromethylbenzanoyl-grafted polyhydroxy graphene oxide (PTFMPA-MHGO, 0.37g).

[0109] Test Example 1.

[0110] FT-IR spectral analysis: Figure 2 The infrared spectra of the products PBPA-MHGO, PCPA-MHGO, and PTFMPA-MHGO from Examples 1, 10, and 11 are shown, with the values ​​located at 1488, 1486, and 1480 cm⁻¹. -1 The absorption peaks are attributed to the stretching vibrations of CN, located at 1632, 1623, and 1615 cm⁻¹. -1 The absorption peak is attributed to the stretching vibration of N=N, indicating the presence of benzene azo groups in the product.

[0111] Test Example 2.

[0112] X-ray diffraction pattern analysis: Figure 3 The X-ray diffraction patterns of the products PBPA-MHGO, PCPA-MHGO, and PTFMPA-MHGO from Examples 1, 10, and 11 are shown in the figures. As can be seen from the figures, compared to MHGO polyhydroxy graphene oxide, the products exhibit new diffraction peaks at 2θ = 9.76°, 9.28°, and 9.24°, corresponding to interlayer spacings of 0.91 nm, 0.95 nm, and 0.96 nm, respectively. This is because the grafting of benzene azo groups onto the MHGO surface increases the average distance between adjacent layers.

[0113] Test Example 3.

[0114] Microwave absorption performance test: The materials obtained in Examples 1, 10, and 11 were uniformly mixed with paraffin at a mass ratio of 2:3, and then pressed into a ring-shaped test sample with an outer diameter of 7.0 mm, an inner diameter of 3.00 mm, and a thickness of 2.00 mm. The sample was then connected to a vector network analyzer, and the microwave absorption performance spectrum and electromagnetic impedance matching spectrum were tested in the frequency range of 2-18 GHz.

[0115] Test results are as follows Figure 4 As shown, Figure 4 The graph in center (ac) shows the correlation between reflection loss and frequency for the ring-shaped test samples. It can be seen that the minimum reflection loss of the polyhydroxy graphene oxide materials grafted with benzene azo groups all exceed the performance requirement of -10 dB defined for microwave absorbing materials. When the thickness is 2.0 mm, PBPA-MHGO achieves a minimum reflection loss of -21.64 dB at 16.24 GHz, with an effective bandwidth of 6.92 GHz. When the thickness is 2.5 mm, PCPA-MHGO achieves a minimum reflection loss of -38.32 dB at 13.26 GHz, with an effective bandwidth of 5.91 GHz. When the thickness is 3.5 mm, PTFMPA-MHGO achieves a minimum reflection loss of -51.17 dB at 10.24 GHz, with an effective bandwidth of 4.84 GHz.

[0116] Figure 4 The graph (df) shows the impedance matching and frequency correlation spectrum of the ring test sample. When the ratio of the input impedance to the free space impedance is |Z... in The closer / Z0| is to 1, the greater the absorption of electromagnetic waves by the material, and the more effectively it dissipates them internally. As shown in the figure, when the thickness is 2.0 mm, the electromagnetic impedance of PBPA-MHGO at 16.24 GHz is 0.82; when the thickness is 2.5 mm, the electromagnetic impedance of PCPA-MHGO at 13.26 GHz is 1.03; and when the thickness is 3.5 mm, the electromagnetic impedance of PTFMPA-MHGO at 10.24 GHz is 0.99. Therefore, grafting phenyl azo groups can effectively adjust the impedance matching of graphene-based materials.

Claims

1. A polyhydroxyapatite-based material grafted with a benzene azo group, characterized in that, The preparation method of this material is as follows: Step 1: Add aniline compounds to dilute hydrochloric acid solution, heat until completely dissolved, and then cool under low temperature conditions; Step 2: Add sodium nitrite solution dropwise to the solution prepared in Step 1, react fully under low temperature conditions, add urea to remove excess sodium nitrite, stir, and obtain diazonium salt; Step 3: Take the polyhydroxy graphene oxide suspension and adjust the pH to 8-10 using an alkaline buffer solution; Step 4: Add the diazonium salt prepared in step 2 to the suspension prepared in step 3, and continue stirring under low temperature conditions to carry out the coupling reaction; Step 5: After the coupling reaction is complete, filter, wash, and vacuum dry to obtain a polyhydroxy graphene oxide-based material grafted with benzene azo groups. In the above steps, the molar ratio of aniline compounds, sodium nitrite, and dilute hydrochloric acid is 1:(1.05~1.15):(2.5~5.5); the molar ratio of aniline compounds to polyhydroxy graphene oxide is 200:

1. In step 1, the aniline compound is p-bromoaniline, p-chloroaniline, or p-trifluoromethylaniline; In step 3, the polyhydroxy graphene oxide suspension is prepared by the following method: 1) Graphene oxide was dispersed in DMSO, manganese acetate was added as a catalyst, and the mixture was stirred until a suspension was formed. The pH was then adjusted to 4 with dilute hydrochloric acid solution. 2) Irradiate the suspension with ultraviolet light for 8 days, add ZnO and isopropanol, and continue to irradiate with ultraviolet light for 8 days to obtain a polyhydroxy graphene oxide suspension.

2. The polyhydroxyapatite-based graphene oxide material grafted with benzene azo groups according to claim 1, characterized in that, The low-temperature conditions are described as being in an ice-water bath at 0~5℃.

3. The polyhydroxyapatite-based graphene oxide material grafted with benzene azo groups according to claim 2, characterized in that, In step 4, the coupling reaction time is 4 to 7 hours.

4. The polyhydroxyapatite-based material grafted with benzene azo groups according to claim 3, characterized in that, in step 1, the concentration of the dilute hydrochloric acid is 4~6 mol / L.

5. The polyhydroxyapatite-based graphene oxide material grafted with benzene azo groups according to claim 4, characterized in that, In step 3, the alkaline buffer solution is a buffer solution prepared from sodium carbonate and sodium bicarbonate.

6. The polyhydroxy graphene oxide-based material grafted with benzene azo groups according to claim 1, characterized in that, in step 4, after the coupling reaction, an appropriate amount of dilute hydrochloric acid is added, the temperature is raised and stirring is continued to remove excess alkaline buffer solution to a pH value of 7; then the temperature is raised to 50°C and stirring is continued for 4 hours to remove byproducts.

7. The polyhydroxy graphene oxide-based material grafted with benzene azo groups according to claim 1, characterized in that, in step 5, the vacuum drying temperature is 80~120℃ and the time is 48 hours.

8. The application of the polyhydroxyapatite-based material grafted with the benzene azo group according to any one of claims 1-7 in microwave absorption.

Citation Information

Patent Citations

  • Synthesis method of p-cyanobenzene azo grafted graphene oxide

    CN116075144A

  • Super-flexible high thermal conductive graphene film and preparation method therefor

    WO2017128648A1

Cited By

  • Ternary heterostructure CoFe2O4 / ZnO-RGO nano composite electromagnetic wave absorbing material as well as preparation method and application thereof

    CN121376994A