Ce-doped Cu and Zn-Al layered bimetallic oxide catalyst for reverse water gas shift and preparation method of Ce-doped Cu and Zn-Al layered bimetallic oxide catalyst

By using Ce doped Cu, Zn-Al layered bimetal oxide catalyst to catalyze the photothermal synergistic catalyzed reverse water gas transformation reaction, the problems of poor selectivity and high energy consumption in the prior art are solved, and the CO2 conversion effect is achieved with high efficiency, stability and low cost.

CN120132862APending Publication Date: 2025-06-13CHENGDU UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510212407.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-25
Publication Date
2025-06-13

AI Technical Summary

Technical Problem

The prior art has problems of poor selectivity and high energy consumption in photothermal synergistic catalytic counterwater gas transformation reaction, and the precious metal catalysts are costly and complex in preparation process, and the non-precious metal catalysts have poor stability.

Method used

The Ce doped Cu, Zn-Al layered bimetal oxide catalyst was prepared by co-precipitation method and aerobic calcination method, which was better than the TiO2 doped catalyst to show a more significant catalytic effect under photothermal conditions.

Benefits of technology

The CO yield with near equilibrium yield at lower catalytic temperatures (450°C) is achieved, with excellent stability and low cost, suitable for industrial conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120132862A_ABST
    Figure CN120132862A_ABST
Patent Text Reader

Abstract

The invention provides a Ce-doped Cu and Zn-Al layered bimetallic oxide catalyst for reverse water gas shift and a preparation method thereof, the catalyst is composed of ZnO, Al2O3, CuO and CeO2, and the mass ratio of ZnO to Al2O3 to CuO to CeO2 is (71-78): (12-15): (5-6): (2-11). According to the preparation method, CeO2 is selected to be doped in layered bimetallic oxide (LDO) formed by calcining Cu-LDH, and compared with TiO2 doping, it is found that CeO2 has a more remarkable catalytic effect compared with TiO2, and the prepared catalyst has excellent stability and can maintain high activity under long-time testing; and the catalyst has CO yield close to equilibrium yield under the condition of relatively low catalytic temperature (450 DEG C), has excellent industrial implementation conversion prospect, and is simple in process steps and suitable for continuous production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts for reverse water-gas shift, and relates to a Ce-doped Cu,Zn-Al layered double metal oxide catalyst for reverse water-gas shift and a preparation method thereof, which are specifically applied to the reverse water-gas shift (RWGS) reaction of catalytically reducing CO 2 to CO under the condition of photo-thermal synergistic catalysis. Background Art

[0002] Catalytically converting CO 2 into valuable chemicals can not only reduce the environmental impact caused by CO 2 emissions, but also provide a sustainable strategy for fuel / chemical production to complete the carbon cycle. Among various CO 2 conversion processes, the direct hydrogenation of CO 2 to methanol is the most ideal conversion strategy. Catalytically reducing CO 2 to CO through the reverse water-gas shift (RWGS) reaction can be a promising alternative for direct methanol production, because CO is an indispensable raw material for producing methanol or other valuable chemicals in the Fischer-Tropsch process. Shoji et al. [1] prepared a series of hydrotalcite-like compounds and applied them to photocatalytic RWGS, but there were many by-products in the catalyst. Therefore, Zhao et al. [2] introduced the photoactive metal Ti into MgAl for photocatalytic RWGS. After 5 h of UV light irradiation, the highest CO yield was only 50 μmol·g Ti -1 , and Chong et al. [3] further loaded Pt / TiO 2 onto the MgAl support for photocatalysis. Although the CO yield was improved to some extent, the problem of poor selectivity was still prominent. This shows that relying solely on pure light energy for catalytic RWGS may lead to problems such as poor selectivity, and may also consume a large amount of energy and cause certain environmental problems [4]. In contrast, photo-thermal synergistic catalysis is a very promising catalytic method. Yang et al. [5] synthesized CuCeO 2 and applied it to catalytic RWGS. The photo-thermal catalytic CO production was 30% higher than that of thermal catalysis, proving that the Cu nanoparticles on the sample surface generated a local surface plasmon resonance (LSPR) effect under light irradiation, accelerating the generation of oxygen vacancies; Wu et al. [6] loaded Ru on Mo 2 TiC 2 , and the CO yield reached an astonishing 4.0 mol·g Ru -1 ·h -1。All of these indicate that the photo-thermal co-catalytic RWGS has received extensive attention as a new "green" catalytic method. However, we note that although noble metals (such as Ru, Rh, Pt, Au, etc.) used in these existing technologies can greatly improve the activation ability of H 2 , due to problems such as high cost, complex preparation process, and easy shedding of low loading, they cannot be directly applied to industrialization in practice; for non-noble metal catalysts (Cu, Ti, Ni, Co, Fe, etc.), although they are proven to have good photoactivity and can generate hot electrons, due to the high loading, they are prone to problems such as carbon deposition and sintering under light irradiation, resulting in poor catalyst stability.

[0003] In summary, if there is a catalyst that is more suitable for photo-thermal co-catalytic reverse water-gas shift reaction and has a lower cost, and at the same time, under the condition of reducing the loading, the CO 2 conversion rate and the CO production rate can be further improved, and certain stability can be maintained, it will be extremely beneficial to further promote the industrial conversion of CO 2 catalytic reduction to CO, and it can be tried to directly apply it to the treatment of industrial tail gas emissions of CO 2 at high temperature. SUMMARY OF THE INVENTION

[0004] In order to solve the above problems in the existing technologies, the present invention provides a Ce-doped Cu, Zn-Al layered double metal oxide catalyst for reverse water-gas shift and its preparation method. CeO 2 is doped into the layered double metal oxide (LDO) formed by calcining Cu-LDH, and compared with that doped with TiO 2 . It is found that CeO 2 has a more significant catalytic effect compared with TiO 2 . The prepared catalyst has excellent stability and can maintain high activity under long-term testing; and has a CO yield close to the equilibrium yield at a relatively low catalytic temperature (450 °C), has excellent industrial implementation and transformation prospects, and at the same time, the process steps are simple and suitable for continuous production.

[0005] To achieve the above object, the present invention is realized by a technical solution composed of the following technical measures.

[0006] On the one hand, the present invention provides a Ce-doped Cu, Zn-Al layered double metal oxide catalyst for reverse water-gas shift, which is composed of ZnO, Al 2 O 3 , CuO and CeO 2 and the mass ratio is (71-78):(12-15):(5-6):(2-11).

[0007] It should be noted that the Ce-doped Cu,Zn-Al layered double metal oxide catalyst uses Cu and Zn as M 2+ and Al as M 3+ . The Ce-doped catalyst is prepared by the co-precipitation method and finally obtained through aerobic calcination. After calcination, the catalyst forms a layered double metal oxide, and the composition and mass ratio of its components are obtained through analysis and calculation by inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0008] On the other hand, the present invention also provides a method for preparing the above-mentioned Ce-doped Cu,Zn-Al layered composite metal oxide catalyst for reverse water gas shift, which mainly includes the following steps:

[0009] (1) Dissolve metal salts of cerium, copper, zinc, and aluminum in deionized water to prepare a mixed metal salt solution, where the molar ratio of Zn / Cu is 9.5 - 10.5, the molar ratio of (Cu + Zn) / Al is 3 - 4, and the molar ratio of Cu / Ce is (1 - 5):1;

[0010] (2) Drop the mixed metal salt solution obtained in step (1) into an alkali metal carbonate buffer solution with a molar concentration of 0.1 - 0.2 mol / L while stirring, and maintain the pH value of the reaction solution at 9.0 - 10.5 by adding a strong base solution during the dropping process. After the dropping is completed, continue stirring for at least 1 h, and then stand for aging until precipitation layering occurs, and separate to obtain an intermediate precipitation product;

[0011] (3) Calcinate the intermediate precipitation product obtained in step (2) in an aerobic atmosphere at 400 - 500 °C for 2 - 5 h to prepare a Ce-doped Cu,Zn-Al layered double metal oxide catalyst.

[0012] In this article, the metal salts of cerium, copper, zinc, and aluminum in step (1) are the selection of conventional metal salt raw materials in metal ion solutions. Those skilled in the art can make specific selections according to the conventional metal salts that can be added to metal ion solutions of cerium, copper, zinc, and aluminum known in the prior art and in combination with actual needs, including but not limited to nitrates, halides, acetates, etc. of cerium, copper, zinc, and aluminum; for simplifying experimental operations and facilitating the design of control experiments, nitrates of cerium, copper, zinc, and aluminum are selected in the specific embodiments of the present invention. Those skilled in the art should clearly recognize that the metal salts of cerium, copper, zinc, and aluminum in step (1) mainly provide metal ions, and the selection of specific anion radicals usually does not affect the technical effects achieved by the present invention. However, it should still be noted that different metal salts may have different solubilities, so there are certain limitations when choosing to use a high-concentration mixed metal salt solution.

[0013] In one of the technical solutions, the metal salts of cerium, copper, zinc, and aluminum in step (1) are nitrates of cerium, copper, zinc, and aluminum.

[0014] It should be added that the molar ratio of Zn / Cu in step (1) is 9.5 - 10.5, and the molar ratio of (Cu + Zn) / Al is 3 - 4. This limits a very narrow range. Firstly, mainly considering that under the condition of maintaining high catalytic activity, the content of the active component Cu should be reduced as much as possible to ensure good stability during subsequent calcination. In addition, when the Cu metal content is too high, lattice expansion may occur, which will affect the formation of the layered structure. Based on the results of variable comparison experiments, the molar ratio of Zn / Cu is limited to 9.5 - 10.5. Secondly, through comparative experiments, it is confirmed that the molar ratio of M 2+ / M 2+ / M 3+ needs to be maintained at 2 - 4 to form a unique layered structure. And based on the specific selection of M 2+ metal and M 3+ metal, the range of its molar ratio is narrowed. Therefore, the molar ratio of (Cu + Zn) / Al is limited to 3 - 4.

[0015] In this article, the alkali metal carbonate buffer solution in step (2) is a carbonate solution of alkali metals commonly used in the chemical industry, such as sodium carbonate solution or potassium carbonate solution.

[0016] It should be noted that since the alkali metal carbonate buffer solution in step (2) mainly plays a buffering role, its addition amount usually does not have an obvious impact on the technical effects achieved by the present invention under appropriate conditions, and those skilled in the art can refer to the addition amount and concentration of conventional buffer solutions in the prior art. To better illustrate the present invention and provide a reference technical solution, the volume ratio of the alkali metal carbonate buffer solution to the metal salt mixed solution in step (2) is (0.16 - 0.25):1.

[0017] In this article, the strong alkali solution in step (2) is a solution prepared by mixing a strong alkali commonly used in the chemical industry with water, such as a solution prepared by mixing sodium hydroxide or potassium hydroxide with water.

[0018] In one of the technical solutions, the molar concentration of the strong alkali solution in step (2) is 0.1 - 0.5 mol / L; its addition method is dropwise addition.

[0019] To accelerate the static aging in step (2), in one of the technical solutions, the static aging is carried out at a temperature of 60 - 75 °C until precipitation and stratification occur.

[0020] In this text, in step (3), the intermediate precipitate obtained in step (2) is calcined at 400-500 °C for 2-5 h in an aerobic atmosphere. It is advisable to wash and dry the precipitate before calcination. However, those skilled in the art should know that the washing and drying of the filtered precipitate are conventional processes in chemical engineering, and those skilled in the art can select appropriate washing and drying methods according to common knowledge or conventional processes by themselves.

[0021] To better illustrate the present invention and provide a reference technical solution, in step (3), the intermediate precipitate obtained in step (2) is calcined at 400-500 °C for 2-5 h in an aerobic atmosphere. Before calcination, the precipitate is washed and dried. The washing is carried out by washing with deionized water at least 3 times to better remove impurity ions in the precipitate; the drying is preferably to dry the washed precipitate at a temperature of 70-100 °C for at least 10 h and keep the drying treatment until calcination.

[0022] In this text, in step (3), the intermediate precipitate obtained in step (2) is calcined at 400-500 °C for 2-5 h in an aerobic atmosphere. The calcination is to convert the metal components in the precipitate into oxides, specifically following the conventional calcination method in chemical engineering. Those skilled in the art can directly refer to the conventional methods for calcining to prepare copper oxide and cerium dioxide for treatment.

[0023] The inventor of the present invention found in the research process that layered double hydroxide (LDH) has been widely used in various photothermal catalytic studies due to its strong tunability, good modification basis, broadening the band gap range of materials, memory effect, and enhancing electron-hole separation. In addition, doping a small amount of tetravalent metal is also an efficient strategy for preparing LDH with high photocatalytic activity, such as Ce 4+ Usually, it can greatly increase the concentration of basic sites in the material, thereby regulating the metal-support interaction. However, some studies have shown that the doping of Ce will bring negative and uncertain factors to the LDH catalyst. Nizio et al. [7] believe that the doping of Ce cannot improve the catalytic activity. Even if the addition of Ce increases the total alkalinity, the Ce-promoted catalyst can only show high activity at relatively high temperatures; some scholars also believe that the doping of Ce will destroy the layered structure of LDH, thereby reducing the specific surface area of LDH [8-9].

[0024] Therefore, in the existing research, the mechanism of action of Ce in the hydrotalcite-like system is highly controversial, and the interaction between Cu and Ce in LDH has not been specifically studied. At the same time, a large number of studies have shown that CeO 2Although it has a relatively wide tunable bandgap, its light absorption is low, especially for visible light. And TiO 2 Under high-temperature and hydrogen-rich conditions, it is more conducive to the formation of TiO 2-x structure, which has a significant light absorption degree. Therefore, it is widely believed that doping TiO 2 Compared with CeO 2 can improve the catalytic performance of the catalyst under light illumination conditions

[10] .

[0025] The inventive point of the present invention lies in that through actual experimental results, it is shown that when CeO 2 is applied to the layered double metal oxide (LDO) formed by calcining Cu-LDH, compared with TiO 2 it has a more significant catalytic effect, which significantly breaks the technical prejudice in the prior art that doping TiO 2 compared with CeO 2 can improve the catalytic performance of the catalyst under photothermal conditions. Through testing and characterization analysis of this phenomenon, it is found that on the one hand, perhaps CeO 2 compared with TiO 2 can better stimulate the LSPR effect of Cu nanoparticles, greatly enhance the light absorption degree of the material and narrow the bandgap, but the specific reason why CeO 2 doped in Cu-LDO is superior to TiO 2 is still unknown for the time being.

[0026] Based on the above research results, in order to further provide sufficient experimental data for industrial implementation and transformation, the research group where the inventors are located has carried out a large number of exploratory experiments on the ratio variable of Cu element and Ce element. In this process, it is surprisingly found that when the molar ratio of Cu element and Ce element is 3:1, the prepared 3Cu1Ce-LDO catalyst shows extremely excellent performance in the photothermal catalytic activity test at 400 °C, and its CO generation rate and CO 2 conversion rate both greatly exceed those of the Ti-doped catalyst under the same conditions.

[0027] In this article, the stirring, dropping, and separation all follow the conventional principles in chemical engineering processes, and those skilled in the art can perform specific operations according to common knowledge.

[0028] The present invention has the following beneficial effects:

[0029] 1. The present invention provides a Ce-doped Cu, Zn-Al layered double metal oxide catalyst for reverse water gas shift and its preparation method. CeO 2 is doped into the layered double metal oxide (LDO) formed by calcining Cu-LDH, and compared with TiO 2Comparing with the doped ones, it is found that CeO 2 Compared with TiO 2 has a more significant catalytic effect, which clearly breaks the technical prejudice in the prior art that doping TiO 2 can improve the catalytic performance of the catalyst under photothermal conditions compared with CeO 2

[0030] 2. The Ce-doped Cu, Zn-Al layered double metal oxide catalyst for reverse water gas shift provided by the present invention has excellent stability and can still maintain its high activity under long-term testing, indicating that the catalyst has good activity stability.

[0031] 3. The Ce-doped Cu, Zn-Al layered double metal oxide catalyst for reverse water gas shift provided by the present invention has an extremely low Cu loading, can effectively reduce costs, and has a CO yield close to the equilibrium yield under relatively low catalytic temperature (450 °C) conditions. It has excellent prospects for industrial implementation and transformation, and at the same time, the process steps are simple and suitable for continuous production. Description of the Drawings

[0032] Figure 1 It is the XRD spectra of the intermediate samples and the finally prepared catalysts of Example 2, Comparative Examples 1-2 of the present invention. Among them, CuCe-LDH refers to the intermediate sample obtained in Example 2, and CuCe-LDO refers to the catalyst sample prepared in Example 2.

[0033] Figure 2 It is the TEM characterization result diagram and energy spectrum scanning result diagram of the finally prepared catalysts of Example 2, Comparative Examples 1-2 of the present invention. Among them, Figure (a) corresponds to the finally prepared catalyst of Comparative Example 2, Figure (b) corresponds to the finally prepared catalyst of Comparative Example 1, and Figure (c) corresponds to the finally prepared catalyst of Example 2; the inserted tables in Figures (b) and (c) are their average particle size distribution tables.

[0034] Figure 3 It is the energy dispersive spectroscopy element distribution diagram of the finally prepared catalysts of Example 2 (right) and Comparative Example 1 (left) of the present invention.

[0035] Figure 4 It is the high-resolution transmission electron microscope diagram of the finally prepared catalysts of Example 2, Comparative Examples 1-2 of the present invention. Among them, Figure (a) corresponds to the finally prepared catalyst of Comparative Example 2, Figure (b) corresponds to the finally prepared catalyst of Comparative Example 1, and Figure (c) corresponds to the finally prepared catalyst of Example 2. Detailed Embodiments

[0036] ​To further understand the present invention, the preferred embodiments of the present invention will be described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention. Those skilled in the art can draw on the content of this article and appropriately modify the process parameters to achieve. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and those skilled in the art can obviously make changes or appropriate modifications and combinations to the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention. Although it is believed that those of ordinary skill in the art are fully aware of the following terms, the following definitions are still stated to help illustrate the subject matter disclosed by the present invention.

[0037] In one aspect, the present invention provides a Ce-doped Cu,Zn-Al layered double metal oxide catalyst for reverse water gas shift, which is composed of ZnO, Al 2 O 3 , CuO and CeO 2 , and the mass ratio is (71-78):(12-15):(5-6):(2-11).

[0038] It should be noted that the Ce-doped Cu,Zn-Al layered double metal oxide catalyst selects Cu and Zn as M 2+ , Al as M 3+ , and the Ce doping is prepared by the co-precipitation method and finally obtained by aerobic calcination. The catalyst forms a layered double metal oxide after calcination, and the composition and mass ratio of its components are obtained through analysis and calculation by inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0039] On the other hand, the present invention also provides a preparation method of the above-mentioned Ce-doped Cu,Zn-Al layered composite metal oxide catalyst for reverse water gas shift, which mainly includes the following steps:

[0040] (1) Dissolve the metal salts of cerium, copper, zinc, and aluminum in deionized water to prepare a mixed metal salt solution, where the elemental molar ratio of Zn / Cu is 9.5-10.5, the elemental molar ratio of (Cu+Zn) / Al is 3-4, and the molar ratio of Cu / Ce is (1-5):1;

[0041] (2) The metal salt mixed solution obtained in step (1) is dropped into an alkali metal carbonate buffer solution with a molar concentration of 0.1 - 0.2 mol / L while stirring, and during the dropping process, the pH value of the reaction solution is maintained at 9.0 - 10.5 by adding a strong base solution. After the dropping is completed, stirring is continued for at least 1 h, and then it is left to age until precipitation stratification occurs, and the intermediate precipitation product is separated;

[0042] (3) The intermediate precipitation product obtained in step (2) is calcined at 400 - 500 °C for 2 - 5 h in an aerobic atmosphere to prepare a Ce-doped Cu, Zn-Al layered double metal oxide catalyst.

[0043] In this article, the metal salts of cerium, copper, zinc, and aluminum in step (1) are the metal salt raw material selections commonly used in metal ion solutions. Those skilled in the art can make specific selections according to the conventional metal salts that can be added to the metal ion solutions of cerium, copper, zinc, and aluminum known in the prior art and in combination with actual requirements. In one of the embodiments, it includes, but is not limited to, nitrates, halides, acetates, etc. of cerium, copper, zinc, and aluminum; for simplifying the experimental operation and facilitating the design of control experiments, nitrates of cerium, copper, zinc, and aluminum are selected in the specific embodiments of the present invention. Those skilled in the art should clearly recognize that the metal salts of cerium, copper, zinc, and aluminum in step (1) mainly provide metal ions, and the selection of the specific anion root usually does not affect the technical effects achieved by the present invention. However, it should still be noted that different metal salts may have different solubilities, so there are certain limitations when choosing to use a high-concentration metal salt mixed solution.

[0044] In one of the embodiments, the metal salts of cerium, copper, zinc, and aluminum in step (1) are nitrates of cerium, copper, zinc, and aluminum.

[0045] It should be supplemented that the molar ratio of the elements Zn / Cu in step (1) is 9.5 - 10.5, and the molar ratio of the elements (Cu + Zn) / Al is 3 - 4. This limits a very narrow range. Firstly, mainly considering that while maintaining high catalytic activity, the content of the active component Cu should be reduced as much as possible to ensure good stability during subsequent calcination. In addition, as Cu is the M 2+ If the metal content is too high, lattice expansion may occur, which will affect the formation of the layered structure. Based on the results of variable comparison experiments, the molar ratio of the elements Zn / Cu is limited to 9.5 - 10.5; secondly, through comparative experiments, it is confirmed that the molar ratio of M 2+ / M 3+ needs to be maintained at 2 - 4 to form a unique layered structure. And based on M 2+ metal and M 3+The specific selection of the metal narrows the range of its molar ratio, so the elemental molar ratio of (Cu + Zn) / Al is limited to 3 to 4.

[0046] In this article, the alkali metal carbonate buffer solution described in step (2) is a carbonate solution of an alkali metal commonly used in the chemical industry. In one embodiment, for example, it is a sodium carbonate solution or a potassium carbonate solution.

[0047] It should be noted that since the alkali metal carbonate buffer solution described in step (2) mainly plays a buffering role, under appropriate conditions, the amount of its addition generally does not significantly affect the technical effects achieved by the present invention, and those skilled in the art can refer to the addition amount and concentration of conventional buffer solutions in the prior art. To better illustrate the present invention and provide a reference embodiment, the volume ratio of the alkali metal carbonate buffer solution to the metal salt mixed solution in step (2) is (0.16 - 0.25):1.

[0048] In this article, the strong base solution described in step (2) is a solution prepared by mixing a strong base commonly used in the chemical industry with water, such as a solution prepared by mixing sodium hydroxide or potassium hydroxide with water.

[0049] In one embodiment, the molar concentration of the strong base solution described in step (2) is 0.1 - 0.5 mol / L; its addition method is dropwise addition.

[0050] To accelerate the static aging in step (2), in one embodiment, the static aging is carried out at a temperature of 60 - 75 °C until precipitation and stratification occur.

[0051] In this article, in step (3), the intermediate precipitate obtained in step (2) is calcined at 400 - 500 °C for 2 - 5 h in an aerobic atmosphere. It is advisable to wash and dry the precipitate before calcination. However, those skilled in the art should know that the washing and drying of the filtered precipitate are conventional processes in the chemical industry, and those skilled in the art can choose appropriate washing and drying methods according to common knowledge or conventional processes.

[0052] To better illustrate the present invention and provide a reference embodiment, in step (3), the intermediate precipitate obtained in step (2) is calcined at 400 - 500 °C for 2 - 5 h in an aerobic atmosphere. Before calcination, the precipitate is washed and dried. The washing is carried out by washing with deionized water at least 3 times to better remove impurity ions in the precipitate; the drying is preferably carried out by drying the washed precipitate at a temperature of 70 - 100 °C for at least 10 h and maintaining the drying treatment until calcination.

[0053] In this paper, in step (3), the intermediate precipitate obtained in step (2) is calcined at 400-500 °C for 2-5 h in an aerobic atmosphere. The calcination converts the metal components in the precipitate into oxides, specifically following the conventional calcination method in the chemical industry. Those skilled in the art can directly refer to the conventional methods for calcining to prepare copper oxide and cerium dioxide for treatment.

[0054] During the research process, the inventors of the present invention found that Layered Double Hydroxide (LDH) has been widely used in various photothermal catalysis studies due to its strong tunability, good modification basis, ability to broaden the bandgap range of materials, memory effect, and enhanced electron-hole separation. In addition, doping a small amount of tetravalent metal is also an efficient strategy for preparing LDH with high photocatalytic activity, such as Ce. 4+ It can usually significantly increase the concentration of basic sites in the material, thereby regulating the metal-support interaction. However, some studies have shown that the doping of Ce will bring negative and uncertain factors to the LDH catalyst. Nizio et al. [7] believe that the doping of Ce cannot improve the catalytic activity. Even if the addition of Ce increases the total alkalinity, the Ce-promoted catalyst can only show high activity at relatively high temperatures. Some scholars also believe that the doping of Ce will damage the layered structure of LDH, thereby reducing the specific surface area of LDH [8-9].

[0055] Therefore, in existing research, the mechanism of action of Ce in the hydrotalcite-like system has been highly debated, and the interaction between Cu and Ce in LDH has not been specifically studied. At the same time, a large number of studies have shown that CeO 2 Although it has a tunable wide bandgap, its light absorption degree is relatively low, especially for visible light absorption, while TiO 2 Under high-temperature and hydrogen-rich conditions, it is more convenient to form TiO 2-x structure, which has a significant light absorption degree. Therefore, it is widely believed that doping TiO 2 compared with CeO 2 can improve the catalytic performance of the catalyst under light irradiation conditions

[10] .

[0056] The inventive point of the present invention is that through actual experimental results, it is shown that when CeO 2 is applied to the layered double metal oxide (LDO) formed by calcining Cu-LDH, compared with TiO 2 it has a more significant catalytic effect, which clearly breaks the technical prejudice in the existing technology that doping TiO 2 compared with CeO 2 can improve the catalytic performance of the catalyst under photothermal conditions. Through testing and characterization analysis of this phenomenon, it is found that on the one hand, perhaps it is CeO2 Compared with TiO 2 It can better stimulate the LSPR effect of Cu nanoparticles, greatly enhance the light absorption degree of the material and narrow the band gap. However, when CeO is doped in Cu-LDO 2 is superior to TiO 2 The specific reason is unknown for the time being.

[0057] Based on the above research results, in order to further provide sufficient experimental data for industrial implementation and transformation, the research group where the inventors are located has carried out a large number of exploratory experiments on the ratio variable of Cu element and Ce element. In this process, it is surprisingly found that when the molar ratio of Cu element and Ce element is 3:1, the prepared 3Cu1Ce-LDO catalyst shows extremely excellent performance in the photothermal catalytic activity test at 400 °C, and its CO generation rate and CO 2 conversion rate both far exceed those of the catalysts doped with Ti under the same conditions.

[0058] In this article, the stirring, dropping, and separation all follow the conventional principles in chemical engineering processes, and those skilled in the art can perform specific operations according to common knowledge.

[0059] The following will further explain the present application with reference to the embodiments. However, those skilled in the art should understand that these embodiments are provided only for the purpose of illustration and are not intended to limit the present application.

[0060] Embodiment

[0061] The following will describe the implementation plan of the present application in detail in combination with the embodiments. However, those skilled in the art will understand that the following embodiments are only used to illustrate the present application and should not be regarded as limiting the scope of the present application. For those not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. Those reagents or instruments not specified by the manufacturer can be obtained through commercial purchases and are conventional products. The present application should not be construed as being limited to the specific embodiments described.

[0062] 1. Raw materials

[0063] Name Purity Supplier <![CDATA[CO 2 > ≥99.99% Chengdu Guoguang Gas Co., Ltd. Ar ≥99.999% Chengdu Guoguang Gas Co., Ltd. Cerium(III) nitrate hexahydrate Analytical reagent Sinopharm Chemical Reagent Co., Ltd. Copper(II) nitrate trihydrate Analytical reagent Sinopharm Chemical Reagent Co., Ltd. Aluminium nitrate nonahydrate Analytical reagent Sinopharm Chemical Reagent Co., Ltd. Zinc nitrate hexahydrate Analytical reagent Sinopharm Chemical Reagent Co., Ltd. Titanium dioxide Analytical reagent Chengdu Kelong Chemical Co., Ltd. Sodium carbonate Analytical reagent Chengdu Kelong Chemical Co., Ltd. Potassium carbonate Analytical reagent Chengdu Kelong Chemical Co., Ltd. Sodium hydroxide Analytical reagent Chengdu Kelong Chemical Co., Ltd.

[0064] 2. Test method

[0065] Thermal catalysis: CO 2The reduction reaction was carried out in a fixed-bed quartz tube reactor. After the calcined catalyst was tableted and sieved, catalyst particles with a mesh size of 40-60 were selected. 0.1 g of the catalyst was weighed and mixed evenly with 0.6 g of quartz sand, and then loaded into the quartz tube. The program temperature controller was turned on, and the temperature was raised to the specified reduction temperature at a heating rate of 10 °C / min. Then, hydrogen was introduced at a flow rate of 20 mL / min to reduce the calcined sample at 400 °C for 1 h. Argon was turned on, and the gas chromatograph was started. After the column oven temperature and the detector temperature reached 80 °C and 140 °C respectively, the TCD detector was turned on, and the bridge current was set to 50 mA. After the reduction was completed, nitrogen was introduced for purging until the reaction temperature was reached, and then the reaction feed gas was turned on to start the reaction.

[0066] Photothermal catalysis: 20 mg of the catalyst sample was taken. The program temperature controller was turned on, and the temperature was raised to the specified reduction temperature at a heating rate of 10 °C / min. Then, H 2 was introduced at a flow rate of 20 mL / min to reduce the calcined sample at 400 °C for 1 h. Argon was turned on, and the gas chromatograph was started. After the column oven temperature and the detector temperature reached 80 °C and 140 °C respectively, the TCD detector was turned on, and the bridge current was set to 50 mA. After the reduction was completed, nitrogen was introduced for purging until the reaction temperature was reached, and then the reaction feed gas was turned on to start the reaction. 1.5 mL / min of CO 2 , 6 mL / min of H 2 and 2.5 mL / min of Ar were charged into the atmospheric pressure photothermal catalysis device. The reaction was carried out for 3 h, and a sample (1 mL) was injected into the gas chromatograph every 0.5 h to detect the contents of carbon monoxide and methane. Among them, a 300 W xenon lamp was used as the light source, and the auxiliary heat temperature was 400 °C. The yields of the photothermal catalytic CO 2 hydrogenation reaction of catalyst samples with different copper-cerium molar ratios were recorded.

[0067] 3. Preparation method

[0068] (1) Nitrates of cerium, copper, zinc, and aluminum were dissolved in deionized water to prepare a 150 mL mixed metal salt solution, where the elemental molar ratio of Zn / Cu was 10, the elemental molar ratio of (Cu + Zn) / Al was 4, the Cu / Ce molar ratio was (1-5):1, and the molar concentration of Cu element was 0.0127 mol / L;

[0069] (2) The mixed metal salt solution obtained in step (1) was dropped into a 25 mL sodium carbonate solution with a molar concentration of 0.15 mol / L while stirring, and the pH value of the reaction solution was maintained at 10 by adding a sodium hydroxide solution with a molar concentration of 0.4 mol / L during the dropping process. After the dropping was completed, stirring was continued for 1 h, and then the mixture was left to age at 65 °C for 3 h. The intermediate precipitate product was obtained by suction filtration and washed and dried;

[0070] (3) Calcinate the intermediate precipitate product obtained in step (2) in an air atmosphere at 400 °C for 4 h to prepare a Ce-doped Cu,Zn-Al layered double metal oxide catalyst.

[0071] Example 1

[0072] Example 1 was carried out according to the steps of the above-mentioned "3. Preparation method". In step (1), the element molar ratio of Cu / Ce was 1:1. The intermediate precipitate product obtained in step (2) during the preparation process was used as an intermediate sample, denoted as 1Cu1Ce-LDH; the finally prepared Ce-doped Cu,Zn-Al layered double metal oxide catalyst was used as a catalyst sample, denoted as 1Cu1Ce-LDO.

[0073] Example 2

[0074] Example 2 was carried out according to the steps of the above-mentioned "3. Preparation method". In step (1), the element molar ratio of Cu / Ce was 3:1. The intermediate precipitate product obtained in step (2) during the preparation process was used as an intermediate sample, denoted as 3Cu1Ce-LDH; the finally prepared Ce-doped Cu,Zn-Al layered double metal oxide catalyst was used as a catalyst sample, denoted as 3Cu1Ce-LDO.

[0075] Example 3

[0076] Example 3 was carried out according to the steps of the above-mentioned "3. Preparation method". In step (1), the element molar ratio of Cu / Ce was 5:1. The intermediate precipitate product obtained in step (2) during the preparation process was used as an intermediate sample, denoted as 5Cu1Ce-LDH; the finally prepared Ce-doped Cu,Zn-Al layered double metal oxide catalyst was used as a catalyst sample, denoted as 5Cu1Ce-LDO.

[0077] Comparative Example 1

[0078] Comparative Example 1 was carried out with reference to the steps of the above-mentioned "3. Preparation method", but cerium nitrate was not added in step (1), that is, in step (1), copper, zinc, and aluminum nitrates were dissolved in deionized water to prepare a 150 mL metal salt mixed solution, where the element molar ratio of Zn / Cu was 10, the element molar ratio of (Cu + Zn) / Al was 4, and the molar concentration of Cu element was 0.0127 mol / L.

[0079] The intermediate precipitate product obtained in step (2) during the preparation process was used as an intermediate sample, denoted as Cu-LDH; the finally prepared Cu,Zn-Al layered double metal oxide catalyst was used as a comparative sample, denoted as Cu-LDO.

[0080] Comparative Example 2

[0081] Comparative Example 2 was prepared by referring to the steps of the above-mentioned "3. Preparation Method", but cerium and copper nitrates were not added in step (1). That is, in step (1), zinc and aluminum nitrates were dissolved in deionized water to prepare a 150 mL metal salt mixed solution, where the molar ratio of Zn / Al elements was 4, and the molar concentration of Zn element was 0.127 mol / L.

[0082] In the preparation process, the intermediate precipitate product obtained in step (2) was used as an intermediate sample, denoted as LDH; the finally prepared Zn-Al layered double metal oxide catalyst was used as a comparative sample, denoted as LDO.

[0083] After the catalysts finally prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were quantitatively analyzed and calculated by a PE Avio 200 type inductively coupled plasma atomic emission spectrometer (ICP-AES), the results are shown in Table 1 below:

[0084] Table 1 Composition and mass fraction of the catalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 2

[0085]

[0086] Comparative Example 3

[0087] Comparative Example 3 is a preparation method of a Ti-doped Cu, Zn-Al layered composite metal oxide catalyst, which mainly includes the following steps:

[0088] (1) Dissolve copper, zinc, and aluminum nitrates and TiO 2 in deionized water to prepare a 150 mL metal salt mixed solution, where the molar ratio of Zn / Cu elements is 10, the molar ratio of (Cu + Zn) / Al elements is 4, the molar ratio of Cu / Ti is 1:1, and the molar concentration of Cu element is 0.0127 mol / L;

[0089] (2) Drop the metal salt mixed solution obtained in step (1) into a 25 mL sodium carbonate solution with a molar concentration of 0.15 mol / L while stirring, and maintain the pH value of the reaction solution at 10 by adding a sodium hydroxide solution with a molar concentration of 0.4 mol / L during the dropping process. After the dropping is completed, continue to stir for 1 h, then stand and age at 65 °C for 3 h, filter to obtain the intermediate precipitate product and wash and dry it. The obtained intermediate precipitate product is used as an intermediate sample, denoted as 1Cu1Ti-LDH;

[0090] (3) Calcinate the intermediate precipitate product obtained in step (2) in an air atmosphere at 400 °C for 4 h to prepare a Ti-doped Cu, Zn-Al layered double metal oxide catalyst as a comparative sample, denoted as 1Cu1Ti-LDO.

[0091] Comparative Example 4

[0092] Comparative Example 4 was prepared according to the preparation method of Comparative Example 3, but the elemental molar ratio of Cu / Ti in step (1) was 3:1. The intermediate precipitate product obtained in step (2) during the preparation process was used as an intermediate sample, denoted as 3Cu1Ti-LDH; the finally prepared Ti-doped Cu, Zn-Al layered double metal oxide catalyst was used as a catalyst sample, denoted as 3Cu1Ti-LDO.

[0093] Comparative Example 5

[0094] Comparative Example 5 was prepared according to the preparation method of Comparative Example 3, but the elemental molar ratio of Cu / Ti in step (1) was 5:1. The intermediate precipitate product obtained in step (2) during the preparation process was used as an intermediate sample, denoted as 5Cu1Ti-LDH; the finally prepared Ti-doped Cu, Zn-Al layered double metal oxide catalyst was used as a catalyst sample, denoted as 5Cu1Ti-LDO.

[0095] The catalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were tested according to the above "2. Test Method", and the results are shown in Tables 2 and 3 below:

[0096] Table 2 Activity test results of the catalyst for photothermal catalysis at 400 °C

[0097]

[0098] Table 3 Activity test results of the catalyst for thermal catalysis at 400 °C

[0099]

[0100] It can be clearly seen that when Cu:Ce = 3:1, it has the best photothermal catalytic activity. By preparing CuTi-LDO with the same molar fraction and molar ratio, it was found that the incorporation of TiO 2 has lower photothermal catalytic activity compared to CeO 2 .

[0101] The chromatographic test data and conversion rates of the 3Cu1Ce-LDO catalyst sample prepared in Example 2 for photothermal at a temperature gradient are summarized in Table 4 below:

[0102] Table 4 Chromatographic test data and conversion rates of 3Cu1Ce-LDH for photothermal at a temperature gradient

[0103]

[0104] As Figure 1(a) is the XRD pattern of the intermediate sample before calcination. For the LDH pattern, it corresponds to the typical ZnAl-LDH peaks, demonstrating the successful preparation of the hydrotalcite phase. By comparing with other intermediate samples, it can be found that all the prepared samples are obvious hydrotalcite phases, indicating that doping does not change the main crystal phase structure. In addition, with the incorporation of Ce, an obvious diffraction peak can be seen at 2θ = 28.55°, which mainly belongs to the diffraction of the (111) crystal plane of Ce in the cerianite CeO 2 phase (PDF#43-1002), which proves the successful introduction of Ce in the intermediate sample. Combining Figure 1 (b) with the fine diffraction peak of the (003) crystal plane of hydrotalcite, it can be seen that with the incorporation of Cu and Ce, the characteristic diffraction peak of hydrotalcite (003) shifts to a lower angle, indicating that the interlayer spacing of hydrotalcite becomes larger at this time, which is related to the changes in the charge density of the layer board and the binding strength between the layer board and the interlayer anions caused by the introduction of Cu and Ce. Figure 1 (c) is the XRD pattern of the intermediate sample after calcination. Since LDH will lose its interlayer H 2 O and the hydroxide dehydrates after calcination, the diffraction peaks after calcination are all in agreement with the synthetic zincite ZnO (PDF#75-1526) phase, and no obvious diffraction peaks of Cu, Al or CuAl 2 O 4 spinel are observed in the diffraction pattern, indicating that their content is low and the distribution is relatively dispersed, making it difficult to form the spinel phase. In addition, according to Bragg's law (2dsinθ = nλ), subtracting the average thickness of the laminate of 0.49 nm, the interlayer spacing D of the three catalysts can be calculated through the (003) diffraction peak. It can be found that after the incorporation of Cu, the interlayer spacing of LDH increases slightly, while the incorporation of Ce leads to a more obvious increase in the interlayer spacing of LDH, mainly due to the influence of the ionic radius. The incorporation of larger and into the LDH sample broadens the interlayer spacing; it may also be caused by the influence of the cation electronegativity: according to the Allred-Rochow scale, Cu (1.75) > Ce (1.08 - 1.23), and the smaller the electronegativity, the greater the expected interlayer spacing. Therefore, the interlayer spacing increases from 0.267 nm to 0.269 nm after the incorporation of Cu, and further doping with Ce increases the interlayer spacing to 0.276 nm. A larger interlayer spacing is expected to expose more active sites, which is helpful for mass transfer during the reaction process.

[0105] Such as Figure 2The results of TEM characterization show that the morphologies of Cu-LDO and CuCe-LDO are both lamellar nanosheet structures with a diameter of about 100 nm. It is found that the lamellar nanosheets of CuCe-LDO are significantly thicker. In addition, obvious CuO nanoparticles can be seen in the TEM image, and the average particle sizes are listed in the table in the figure. The results indicate that the incorporation of Ce increases the particle size of CuO nanoparticles, which is mainly attributed to CeO 2 promotes the coalescence of smaller CuO particles into larger particles, which is the result of solid-state diffusion. It also shows that Ce enters the main lattice of CuO, thus forming a solid solution phase, which helps to generate the Cu-O-Ce interface structure. The catalysts were subjected to energy spectrum scanning, and obvious distributions of Zn, Al, Cu, and O elements can be observed in both figures. The distribution of Ce element can be observed in CuCe-LDO, and the distribution of each element is relatively uniform, which corroborates the successful synthesis of layered oxides (LDO). Comparing the mapping diagrams of the two ( Figure 3 ), it can be found that CuCe-LDO has a higher content of surface oxygen species, indicating that the addition of Ce is beneficial to the formation of surface oxygen. After Ce doping, the Cu content on the catalyst surface is lower. Combining with the XRD characterization analysis, this is mainly due to the formation of a solid solution phase by the incorporation of Ce, which weakens the Ce-O bond and thus promotes the exposure of surface oxygen, which is beneficial to the formation of oxygen vacancies. From the HRTEM diagram ( Figure 4 ), multiple sets of lattice fringes are observed and oriented at an angle of 120° relative to each other, which also confirms the hexagonal layered hydrotalcite structure. This lattice spacing can reflect the surface structure of layered hydrotalcite. Calculating the interplanar spacing, it is found that the surface interplanar spacings of the catalysts LDO, Cu-LDO, and CuCe-LDO are 0.267 nm, 0.269 nm, and 0.276 nm, respectively, which is in good agreement with the layer spacing calculated above.

[0106] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited by the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement methods and are all included in the protection scope of the present invention.

[0107] The references cited in the present invention are as follows:

[0108] [1]Shoji I, Kentaro T, Saburo H, et al. Photocatalytic conversion of CO 2in an aqueous solution using various kinds of layered double hydroxides[J].Catalysis Today,2015,215:140-144.

[0109] [2]Zhao H L,Xu J Y,Liu L J,et al.CO 2 photoreduction with water vaporby Ti-embedded MgAl layered double hydroxides[J].Journal of CO 2 Utilization,2016,15:15-23.

[0110] [3]Chong R F,Su C H,Du Y Q,et al.Insights into the role of MgAllayered double oxides interlayer in Pt / TiO 2 toward photocatalytic CO 2 reduction[J].Journal of Catalysis,2018,363:92-101.

[0111] [4]Wang SH,Tountas AA,Pan WB,Zhao JJ,He L,Sun W,et al.CO 2 Footprintof Thermal Versus Photothermal CO2 Catalysis.Small 2021.

[0112] [5]Yang Z,Zeng M,Wang K,et al.Visible light-assisted thermalcatalytic reverse water gas reaction over Cu-CeO 2 :The synergistic of hotelectrons and oxygen[J].Fuel,2022,315:123186.

[0113] [6]Wu Z Y,Shen J H,Li C R,et al.Mo 2 TiC2 MXene-Supported Ru Clusters for Efficient Photothermal Reverse Water-Gas Shift[J]. ACS Nano, 2022, 17(2): 1550-1559.

[0114] [7] Nizio M, Benrabbah R, Krzak M, et al. Low temperature hybrid plasma-catalytic methanation over Ni-Ce-Zr hydrotalcite-derived catalysts[J]. Catalysis Communications, 2016, 83: 14-17.

[0115] [8] Daza C E, Moreno S, Molina R. Co-precipitated Ni-Mg-Al catalysts containing Ce for CO reforming of methane[J]. International Journal of Hydrogen Energy, 2011, 36: 3886-3894.

[0116] [9] Daza C E, Gallego J, Mondragón F, et al. High stability of Ce-promoted Ni / Mg-Al catalysts derived from hydrotalcites in dry reforming of methane[J]. Fuel, 2010, 89: 592-603.

[0117]

[10] Rodriguez J A, Liu P, Wang X, et al. Water-gas shift activity of Cu surfaces and Cu nanoparticles supported on metal oxides[J]. Catalysis Today, 2009, 143: 45-50.

Claims

1. A Ce-doped Cu, Zn-Al layered bimetallic oxide catalyst for reverse water gas shift, characterized in that It is composed of ZnO, Al2O3, CuO and CeO2, and the mass ratio is (71-78):(12-15):(5-6):(2-11).

2. A method for preparing a Ce-doped Cu, Zn-Al layered composite metal oxide catalyst for reverse water gas shift, characterized in that The main steps include: (1) dissolving metal salts of cerium, copper, zinc and aluminum in deionized water to prepare a metal salt mixed solution, wherein the element molar ratio of Zn / Cu is 9.5-10.5, the element molar ratio of (Cu+Zn) / Al is 3-4, and the element molar ratio of Cu / Ce is (1-5):1; (2) adding the metal salt mixed solution obtained in step (1) dropwise to an alkali metal carbonate buffer solution having a molar concentration of 0.1 to 0.2 mol / L while stirring, and maintaining the pH value of the reaction solution at 9.0 to 10.5 by adding a strong alkali solution during the dropping process. After the dropping is completed, stirring is continued for at least 1 hour, and then allowed to stand for aging until precipitation and stratification occur, and an intermediate precipitate product is separated; (3) The intermediate precipitate product obtained in step (2) is calcined at 400-500° C. for 2-5 h in an oxygen atmosphere to prepare a Ce-doped Cu, Zn-Al layered bimetallic oxide catalyst.

3. The preparation method according to claim 2, characterized in that: The metal salts of cerium, copper, zinc and aluminum in step (1) are nitrates of cerium, copper, zinc and aluminum.

4. The preparation method according to claim 2, characterized in that: The alkali metal carbonate buffer solution in step (2) includes sodium carbonate solution or potassium carbonate solution; the volume ratio of the alkali metal carbonate buffer solution to the metal salt mixed solution in step (2) is (0.16-0.25):

1.

5. The preparation method according to claim 2, characterized in that: The molar concentration of the strong alkaline solution in step (2) is 0.1 to 0.5 mol / L.

6. The preparation method according to claim 2, characterized in that: The static aging in step (2) is carried out at a temperature of 60 to 75° C. until precipitation and stratification occur.

7. Use of the Ce-doped Cu, Zn-Al layered bimetallic oxide catalyst as claimed in claim 1 in the reverse water gas shift reaction.

Citation Information

Cited By

  • Lanthanum-doped CuMgAl catalyst as well as preparation method and application thereof

    CN120861113A

  • La-doped CuMgAl catalyst, its preparation method and application

    CN120861113B