Titanium-based ceramic target material and preparation method and application thereof

Titanium-based ceramic targets are prepared by multi-element co-doping and atmospheric pressure sintering. The titanium-based film produced by sputtering forms a stacked structure with the ITO film, which solves the problems of scarce resources and high cost of traditional transparent conductive films, and realizes the preparation of high-performance transparent conductive layers, which is suitable for the solar cell field.

CN120136541APending Publication Date: 2025-06-13LUOYANG JINGLIAN OPTOELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510298229.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-13
Publication Date
2025-06-13

AI Technical Summary

Technical Problem

In the prior art, traditional transparent conductive films such as ITO are scarce indium resources and expensive, and doped materials are difficult to take into account both high conductivity and high light transmittance during the sintering process, and the interfacial energy level mismatch problem, and the high-pressure sintering process is high and the process is complex, making it difficult to achieve large-scale production.

Method used

Through the coordinated doping of multi-elements and dynamic regulation of the sintering atmosphere, titanium-based ceramic targets were prepared by the normal pressure sintering method. The sputtered titanium-based film formed a laminated structure with the ITO film, achieving high conductivity, high light transmittance and high electron mobility.

Benefits of technology

It has achieved high performance preparation of titanium-based ceramic targets. The titanium-based film and ITO film stacked structure have high conductivity, high light transmittance and high electron mobility, and is suitable for silicon-based and perovskite solar cells.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a titanium-based ceramic target material and a preparation method and application thereof.The titanium-based ceramic target material is prepared from, by mass, 96.4 wt%-98.3 wt% of titanium oxide and 1.7 wt%-3.6 wt% of doped oxide, and the doped oxide is prepared from, by mass, 0.8 wt%-1.5 wt% of niobium oxide, 0.5 wt%-1.0 wt% of tantalum oxide, 0.3 wt%-0.8 wt% of tungsten oxide and 0.1 wt%-0.3 wt% of aluminum oxide. According to the method, the high-performance titanium-based ceramic target material is prepared by adopting a normal-pressure sintering method through multi-element synergistic doping and dynamic regulation and control of the sintering atmosphere, the titanium-based thin film prepared by sputtering the titanium-based ceramic target material can form a laminated thin film structure with an indium tin oxide (ITO) thin film, and high conductivity, high visible light transmittance and high electron mobility are achieved; and the actual requirements in the field of silicon-based and perovskite solar cells are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional ceramic materials for sputtering transparent conductive films of solar cells, and specifically relates to a titanium-based ceramic target, a preparation method thereof, and an application thereof. Background Art

[0002] Due to the scarcity and high cost of indium resources in traditional transparent conductive films (such as ITO), it is urgent to develop indium-free alternative materials. Titanium oxide (TiO 2 ) as an ideal candidate material for the transparent conductive layer of solar cells has good light transmittance and chemical stability, but pure TiO 2 has poor conductivity and its conductivity needs to be improved by doping and sintering. In the prior art, single-element doping (such as Nb-TiO 2 , Ta-TiO 2 ) is often accompanied by grain coarsening, making it difficult to balance the high conductivity and high light transmittance of the film, and there are also interface energy level mismatch problems when laminated with ITO; multi-element doping often sacrifices the titanium content, and this high doping content leads to increased light absorption and reduced electron mobility of the film layer. In addition, traditional high-pressure sintering processes (such as hot pressing / SPS) are costly and complex, and it is difficult to achieve large-scale production; and it is difficult to control the oxygen vacancy concentration during the sintering process, resulting in a decrease in the light transmittance of the film layer. Summary of the Invention

[0003] In order to solve the deficiencies in the prior art, the present invention provides a titanium-based ceramic target, a preparation method thereof, and an application thereof. The present invention prepares a high-performance titanium-based ceramic target by multi-element co-doping and dynamic regulation of the sintering atmosphere, and uses an atmospheric pressure sintering method. The titanium-based film obtained by sputtering the titanium-based ceramic target can form a laminated film structure with indium tin oxide (ITO) film, which has high conductivity, high visible light transmittance and high electron mobility, meeting the actual requirements in the fields of silicon-based and perovskite solar cells.

[0004] In order to achieve the above object, the specific solutions adopted by the present invention are as follows: On the one hand, the present invention discloses a titanium-based ceramic target. In terms of mass fraction, the titanium-based ceramic target comprises 96.4 - 98.3 wt% of titanium oxide and 1.7 - 3.6% of doped oxide. Among them, the components included in the doped oxide and the mass fraction of each component are: niobium oxide 0.8 - 1.5 wt%, tantalum oxide 0.5 - 1.0 wt%, tungsten oxide 0.3 - 0.8 wt%, and aluminum oxide 0.1 - 0.3 wt%.

[0005] On the other hand, the present invention discloses a preparation method of a titanium-based ceramic target, which mainly includes the following steps: Step 1: Place the titanium oxide powder and the doped oxide powder in a high-speed disperser for dispersion to obtain a mixed material. Then, formulate an aqueous slurry by mixing the mixed material, ultrapure water, a dispersant, and a binder, and perform sufficient ball milling. Step 2: Spray-dry the aqueous slurry to obtain a powder; then press the powder into a green body. Step 3: Perform atmospheric sintering according to the following stages: (1) Low-temperature stage: In an air atmosphere or an oxygen-nitrogen mixed atmosphere with an oxygen content of 15 - 25%, first heat from room temperature to 300°C at a heating rate of 0.5°C / min, then heat to 550°C at a heating rate of 0.1°C / min, then heat to 750°C at a heating rate of 0.05°C / min, hold at 750°C for 6 h, and finally heat to 1000°C at a heating rate of 0.5°C / min. (2) Medium-temperature stage: In an oxygen-nitrogen mixed atmosphere with an oxygen content of 40 - 60%, first hold at 1000°C for 5 h, and then heat to 1350 - 1430°C at a heating rate of 0.5°C / min. (3) High-temperature stage: Hold at 1350 - 1430°C for 9 - 20 h, divided into three stages according to the holding time, each stage lasting 2 - 7 h. The first and third stages are carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 40 - 60%, while the second stage is carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 15 - 25%. (4) Cooling stage: In a pure oxygen atmosphere, first cool to 1000°C at a cooling rate of 0.5°C / min, and then cool to 800°C at a cooling rate of 0.3°C / min. (5) Annealing stage: In an inert atmosphere, first hold at 800°C for 1 - 2 h, then cool to 600°C at a cooling rate of 1°C / min, hold at 600°C for 1 - 2 h, and then cool to room temperature with the furnace, thus obtaining the titanium-based ceramic target.

[0006] Further, in Step 1, the addition amount of ultrapure water is added according to 50 - 60 wt% of the solid content of the slurry, the addition amount of the dispersant is 1.0 - 1.5 wt% of the total mass of the mixed material, and the addition amount of the binder is 1.5 - 2.5 wt% of the total mass of the mixed material.

[0007] Further, in Step 1, the dispersant is one or more of polycarboxylates, ammonium polyacrylate, citrate salts, polyvinylpyrrolidone, and cetyltrimethylammonium bromide.

[0008] Further, in Step 1, the binder is one or more of polyvinyl alcohol, polyethylene glycol - 1000, polymethacrylic acid, and carboxymethyl cellulose.

[0009] Further, in Step 1, the D50 of the titanium dioxide powder is 0.8 μm, and the particle size of the doped oxide powder is not greater than 200 nm.

[0010] Further, in Step 2, the powder material is placed in a mold, first dry-pressed into shape under a pressure of 80 MPa, and then cold isostatically pressed under a pressure of 300 MPa. The density of the obtained green body is greater than 60%.

[0011] On the other hand, the present invention discloses an application of a laminated film prepared from a titanium-based ceramic target in silicon-based and perovskite solar cells.

[0012] Further, the laminated film is composed of a titanium-based film and an ITO film deposited on the surface of the titanium-based film. Among them, the titanium-based film is obtained by sputtering a titanium-based ceramic target, and the ITO film is obtained by sputtering an ITO target.

[0013] Further, the substrate is placed on the base of the sputtering coater. First, a titanium-based film with a thickness of 50 nm is deposited by DC sputtering using a titanium-based ceramic target under the condition that the substrate temperature is 180 °C; then an ITO film with a thickness of 50 nm is deposited by RF sputtering using an ITO target under the condition that the substrate temperature is 200 °C.

[0014] Beneficial effects: (1) The titanium-based ceramic target provided by the present invention adopts multi-element coordinated doping, and its components are 96.4 - 98.3 wt% of titanium dioxide (TiO 2 ), and 1.7 - 3.6 wt% of doped oxide; the doped oxide is niobium oxide (Nb 2 O 5 ), tantalum oxide (Ta 2 O 5 ), tungsten oxide (WO 3 ), aluminum oxide (Al 2 O 3 ). Among them, niobium oxide (0.8 - 1.5 wt%) is used as a donor dopant to replace Ti 4+ to release free electrons and increase the carrier concentration. Tantalum oxide (0.5 - 1.0 wt%) is used as a grain boundary regulator, and Ta 5+ segregates at the grain boundary to inhibit abnormal grain growth. Tungsten oxide (0.3 - 0.8 wt%) is used as a shallow energy level defect former to reduce electron scattering and increase the electron mobility. Aluminum oxide (0.1 - 0.3 wt%) is used as a sintering aid to promote sintering densification. In addition, tantalum oxide can form a composite doping with aluminum oxide at the grain boundary position, which can generate high-mobility grain boundaries. The grain boundary width is reduced to less than 2 nm, and the grain boundary barrier height is reduced to less than 0.1 eV, achieving the beneficial effect of reducing the carrier transport resistance.

[0015] (2) During the atmospheric pressure sintering process of the present invention, the atmosphere is dynamically adjusted. Among them, a mixed oxygen-nitrogen atmosphere with a low oxygen content is used in the low-temperature stage to slow down the surface diffusion rate, avoid the premature generation of closed pores, inhibit premature densification, and reduce impurity residues. A mixed oxygen-nitrogen atmosphere with a high oxygen content is used in the medium-temperature stage to inhibit the generation and maintain the stable state of Ti 3+ formation and maintenance of Ti 4+ stable state, reduce lattice distortion, and promote uniform grain growth; reasonably control the pre-generation of oxygen vacancies to provide an appropriate carrier concentration. In the initial stage of the high-temperature stage, a mixed oxygen-nitrogen atmosphere with a high oxygen content is used to promote surface diffusion, eliminate closed pores, and is beneficial to improving the sintering density of the target; then reducing the oxygen content can induce the generation of oxygen vacancies and significantly increase the carrier concentration; finally, increasing the oxygen content back to a high level can fill some of the excessive oxygen vacancies to balance the conductivity and light transmittance. Switching to a pure oxygen atmosphere in the cooling stage can partially fill the excessive oxygen vacancies generated in the high-temperature stage, avoiding deep-level defects caused by excessive generation of Ti 3+ ; and pure oxygen can penetrate into the grain boundaries to repair the lack of lattice oxygen, reduce grain boundary scattering, and lower the grain boundary barrier. An inert atmosphere is used in the annealing stage to prevent the material surface from reacting with oxygen to form non-stoichiometric oxides during the cooling process, and rapid annealing and cooling can stabilize the sintering state in the high-temperature stage and maintain the segregation distribution of grain boundary doping elements (Ta, W, Al), thereby reducing the grain boundary resistance.

[0016] (3) A multi-element synergistic doping system of Nb, Ta, W, and Al is used to optimize carrier transport, forming shallow-level composite donor centers, which is beneficial to increasing the electron mobility to more than 25 cm² / V·s; through the dynamic adjustment mechanism of the mixed oxygen-nitrogen atmosphere during atmospheric pressure sintering, the oxygen partial pressure is controlled in stages and multiple times in the high-temperature stage of atmospheric pressure sintering, and the oxygen vacancy concentration is controlled at 10 17 -10 18 cm -3 to avoid light absorption loss; the grain size is controlled by the grain boundary engineering of the segregation of doping elements such as Ta and Al, restricting the abnormal growth of grain size and forming high-mobility grain boundaries; the relative density of the obtained titanium-based ceramic target is above 98.6%, the resistivity is lower than 5×10 -4 Ω•cm, and the average grain size is 8±1 μm. The titanium-based thin film prepared by sputtering the above titanium-based ceramic target has a high electron mobility. When forming a stacked film with a conventional ITO thin film, it can alleviate the interface energy level mismatch problem, reduce interface recombination, and meet the actual requirements of the transparent conductive layer in the fields of silicon-based and perovskite solar cells. Detailed implementation manners

[0017] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0018] First, the present invention provides a titanium-based ceramic target material, which, by mass fraction, comprises 96.4-98.3wt% titanium oxide and 1.7-3.6wt% doped oxides; the doped oxides are niobium oxide, tantalum oxide, tungsten oxide, and aluminum oxide. Niobium oxide (0.8-1.5wt%) is used as a donor dopant to replace Ti 4+ Release free electrons and increase carrier concentration. Tantalum oxide (0.5-1.0wt%), as a grain boundary regulator, Ta 5+ Segregation at grain boundaries inhibits abnormal grain growth. Tungsten oxide (0.3-0.8wt%) acts as a shallow level defect former to reduce electron scattering and improve electron mobility. Alumina (0.1-0.3wt%) acts as a sintering aid to promote sintering densification.

[0019] Secondly, the preparation method of the titanium-based ceramic target mainly includes the following steps: Step 1: Use 4N grade rutile phase titanium oxide powder (D50=0.8μm), niobium oxide nanopowder, tantalum oxide nanopowder, tungsten oxide nanopowder, and aluminum oxide nanopowder (niobium oxide nanopowder, tantalum oxide nanopowder, tungsten oxide nanopowder, and aluminum oxide nanopowder to form doped oxides with a particle size of no more than 200nm) and disperse them in a high-speed disperser for 12 hours to obtain a mixture. Then, the mixture, ultrapure water, dispersant, and binder are prepared into a water-based slurry and fully ball-milled. The ultrapure water is added The amount is added according to the solid content of the slurry being 50-60wt%, the amount of the dispersant added is 1.0-1.5wt% of the total mass of the mixture, and the amount of the binder added is 1.5-2.5wt% of the total mass of the mixture. Specifically, the dispersant is one or more of polycarboxylates, ammonium polyacrylates, citrates, polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, etc.; the binder is one or more of polyvinyl alcohol, polyethylene glycol-1000, polymethacrylic acid, carboxymethyl cellulose, etc.; Step 2: spray-dry the water-based slurry to obtain a powder; then place the powder in a mold, first dry-press it at a pressure of 80 MPa, and then cold isostatically press it at a pressure of 300 MPa to obtain a green body, wherein the density of the green body is greater than 60%; Step 3: Perform pressureless sintering in the following stages: (1)Low - temperature stage: In an air atmosphere or an oxygen - nitrogen mixed atmosphere with an oxygen content of 15 - 25%, first heat from room temperature to 300°C at a heating rate of 0.5°C / min, then heat to 550°C at a heating rate of 0.1°C / min, then heat to 750°C at a heating rate of 0.05°C / min, hold at 750°C for 6 h, and finally heat to 1000°C at a heating rate of 0.5°C / min; (2)Medium - temperature stage: In an oxygen - nitrogen mixed atmosphere with an oxygen content of 40 - 60%, first hold at 1000°C for 5 h, then heat to 1350 - 1430°C at a heating rate of 0.5°C / min; (3)High - temperature stage: Hold at 1350 - 1430°C for 9 - 20 h, divided into three stages according to the holding time, each stage lasts for 2 - 7 h. The first and third stages are carried out in an oxygen - nitrogen mixed atmosphere with an oxygen content of 40 - 60%, while the second stage is carried out in an oxygen - nitrogen mixed atmosphere with an oxygen content of 15 - 25%; (4)Cooling stage: In a pure oxygen atmosphere, first cool to 1000°C at a cooling rate of 0.5°C / min, then cool to 800°C at a cooling rate of 0.3°C / min; (5)Annealing stage: In an inert atmosphere, first hold at 800°C for 1 - 2 h, then cool to 600°C at a cooling rate of 1°C / min, hold at 600°C for 1 - 2 h, and then cool to room temperature with the furnace, thus obtaining the titanium - based ceramic target.

[0020] Furthermore, the present invention discloses a method for preparing a laminated film using the above - mentioned titanium - based ceramic target, which mainly includes the following steps: (1)Place the substrate on the base of the sputtering coater, and deposit a titanium - based thin film with a thickness of 50 nm on the substrate at a substrate temperature of 180°C by DC sputtering (power 150 W, Ar / O 2 =9:1) using the titanium - based ceramic target; (2)Deposit an ITO thin film with a thickness of 50 nm by RF sputtering using an ITO target (In 2 O 3 :SnO 2 =90:10 wt%) at a substrate temperature of 200°C.

[0021] The laminated film prepared by the method of the present invention has good applications in silicon - based and perovskite solar cells.

[0022] Example 1 This example provides a method for preparing a laminated film, which mainly includes the following steps: S1. Prepare the titanium - based ceramic target S11. Raw material mixing and grinding: Take 97.2 wt% of 4N rutile titanium oxide powder (D50 = 0.8 μm), 1.2 wt% of niobium oxide powder, 0.8 wt% of tantalum oxide powder, 0.6 wt% of tungsten oxide powder, and 0.2 wt% of alumina powder (the particle size of the doped oxide ≤ 200 nm) by mass fraction. Place them together in a high-speed disperser and disperse for 12 h. Then, take the mixed material, ultrapure water, polycarboxylate dispersant, and polyvinyl alcohol binder to prepare an aqueous slurry together, and ball mill for 10 h. The addition amount of ultrapure water is added according to 55 wt% of the slurry solid content. The addition amount of polycarboxylate dispersant is 1.2 wt% of the total mass of the mixed material, and the addition amount of polyvinyl alcohol binder is 1.5 wt% of the total mass of the mixed material; S12. Powder granulation and forming: Spray-dry the aqueous slurry to obtain powder; place the powder in a mold, first perform dry pressing at a pressure of 300 MPa, and then perform cold isostatic pressing at a pressure of 300 MPa to obtain a green body. The density of the obtained green body is greater than 60%; S13. Carry out atmospheric sintering according to the following stages: (1) Low-temperature stage: In an air atmosphere or an oxygen-nitrogen mixed atmosphere with 20% oxygen content, first heat from room temperature to 300 °C at a heating rate of 0.5 °C / min, then heat to 550 °C at a heating rate of 0.1 °C / min, then heat to 750 °C at a heating rate of 0.05 °C / min, and hold at 750 °C for 6 h. Finally, heat to 1000 °C at a heating rate of 0.5 °C / min; (2) Medium-temperature stage: In an oxygen-nitrogen mixed atmosphere with 50% oxygen content, first hold at 1000 °C for 5 h, and then heat to 1350 °C at a heating rate of 0.5 °C / min; (3) High-temperature stage: Hold at 1350 °C for 12 h, divided into three stages according to the holding time, each stage lasts for 4 h. The first and third stages are carried out in an oxygen-nitrogen mixed atmosphere with 50% oxygen content, while the second stage is carried out in an oxygen-nitrogen mixed atmosphere with 20% oxygen content; (4) Cooling stage: In a pure oxygen atmosphere, first cool to 1000 °C at a cooling rate of 0.5 °C / min, and then cool to 800 °C at a cooling rate of 0.3 °C / min; (5) Annealing stage: In an inert atmosphere, first hold at 800 °C for 2 h, then cool to 600 °C at a cooling rate of 1 °C / min, hold at 600 °C for 2 h, turn off the heat source below 600 °C and cool naturally in the furnace in an inert atmosphere to obtain the titanium-based ceramic target; S2. Preparation of laminated film S21. Place the substrate on the base of the sputtering coater, and use the titanium-based ceramic target to perform DC sputtering (power 150 W, Ar / O 2=9: 1) Deposit a titanium-based thin film with a thickness of 50 nm at a substrate temperature of 180 °C. S22. Use an ITO target (In2O3:SnO2 = 90:10 wt%) to deposit an ITO thin film with a thickness of 50 nm by RF sputtering at a substrate temperature of 200 °C.

[0023] After testing, the relative density of the titanium-based ceramic target obtained in this example is 98.8%, the grain size is 8.5 μm, and the resistivity is 4.5×10 -4 Ω•cm. The resistivity of the obtained titanium-based thin film is 8.5×10 -4 Ω•cm, the light transmittance of the film layer is 89%, and the electron mobility is 26 cm² / V·s; the resistivity of the obtained ITO thin film is 1.8×10 -4 Ω•cm, the light transmittance of the film layer is 92%, and the electron mobility is 35 cm² / V·s; the resistivity of the obtained laminated thin film is 6.5×10 -4 Ω•cm, the light transmittance of the film layer is 88%, and the electron mobility is 30 cm² / V·s.

[0024] Example 2 The differences between Example 2 and Example 1 are as follows: 1) In step S11, in terms of mass fraction, take 97.8 wt% of 4N grade rutile phase titanium oxide powder (D50 = 0.8 μm), 0.8 wt% of niobium oxide powder, 1.0 wt% of tantalum oxide powder, 0.3 wt% of tungsten oxide powder, and 0.1 wt% of alumina powder (doped nanopowder particle size ≤ 200 nm); 2) In step S13, (2) Medium temperature stage: In an oxygen-nitrogen mixed atmosphere with an oxygen content of 50%, first keep the temperature at 1000 °C for 5 h, and then increase the temperature to 1430 °C at a heating rate of 0.5 °C / min; (3) High temperature stage: Keep the temperature at 1430 °C for 12 h, divided into three stages according to the holding time, each stage lasts for 4 h, the first and third stages are carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 50%, and the second stage is carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 20%.

[0025] The relative density of the obtained titanium-based ceramic target is 98.6%, the grain size is 8.8 μm, and the resistivity is 4.8×10 -4 Ω•cm. The resistivity of the obtained titanium-based thin film is 9.0×10 -4 Ω•cm, the light transmittance of the film layer is 91%, and the electron mobility is 24 cm² / V·s; the resistivity of the obtained ITO thin film is 2.0×10 -4 Ω•cm, the light transmittance of the film layer is 93%, and the electron mobility is 32 cm² / V·s; the resistivity of the obtained laminated thin film is 7.4×10 -4 Ω•cm, the light transmittance of the film layer is 90%, and the electron mobility is 28 cm² / V·s.

[0026] Example 3 Example 3 is different from Example 1 in the following aspects: 1) In step S11, in terms of mass fraction, 97 wt% of 4N grade rutile titanium oxide powder (D50 = 0.8 μm), 1.5 wt% of niobium oxide powder, 0.5 wt% of tantalum oxide powder, 0.8 wt% of tungsten oxide powder, and 0.2 wt% of alumina powder (doped nanopowder particle size ≤ 200 nm) are taken; 2) In step S13, (2) Medium-temperature stage: In an oxygen-nitrogen mixed atmosphere with an oxygen content of 50%, first keep the temperature at 1000 °C for 5 h, and then increase the temperature to 1400 °C at a heating rate of 0.5 °C / min; (3) High-temperature stage: Keep the temperature at 1400 °C for 12 h. According to the holding time, it is divided into three stages, each stage lasting for 4 h. The first and third stages are carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 50%, while the second stage is carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 20%.

[0027] The relative density of the obtained titanium-based ceramic target is 99.1%, the grain size is 7.5 μm, and the resistivity is 3.8×10 -4 Ω•cm. The resistivity of the obtained titanium-based thin film is 7.2×10 -4 Ω•cm, the light transmittance of the film layer is 87%, and the electron mobility is 28 cm² / V·s; the resistivity of the obtained ITO thin film is 1.6×10 -4 Ω•cm, the light transmittance of the film layer is 90%, and the electron mobility is 38 cm² / V·s; the resistivity of the obtained laminated thin film is 5.2×10 -4 Ω•cm, the light transmittance of the film layer is 86%, and the electron mobility is 35 cm² / V·s.

[0028] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that in step S11, in terms of mass fraction, 100 wt% of 4N grade rutile titanium oxide powder (D50 = 0.8 μm) is taken.

[0029] The relative density of the obtained titanium oxide target is 92.1%, the grain size is 14.5 μm, and the resistivity is 5.8×10 2 Ω•cm. The resistivity of the obtained titanium oxide thin film is 8.5×10 2 Ω•cm, the light transmittance of the film layer is 35%, and the electron mobility is 6 cm² / V·s; the resistivity of the obtained ITO thin film is 1.6×10 -4 Ω•cm, the light transmittance of the film layer is 92%, and the electron mobility is 34 cm² / V·s. The resistivity of the obtained laminated thin film is 1.5×10 -1 Ω•cm, the light transmittance of the film layer is 83%, and the electron mobility is 8 cm² / V·s.

[0030] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is as follows: in step S11, in terms of mass fraction, 98.5 wt% of 4N rutile titanium oxide powder (D50 = 0.8 μm) and 1.5 wt% of niobium oxide powder (doped nanopowder particle size ≤ 200 nm) are taken.

[0031] The relative density of the obtained titanium-based ceramic target is 95.1%, the grain size is 12.5 μm, and the resistivity is 1.2×10 -2 Ω•cm. The resistivity of the obtained titanium-based thin film is 1.8×10 -2 Ω•cm, the light transmittance of the film layer is 82%, and the electron mobility is 16 cm² / V·s; the resistivity of the obtained ITO thin film is 1.6×10 -4 Ω•cm, the light transmittance of the film layer is 90%, and the electron mobility is 31 cm² / V·s; the resistivity of the obtained laminated thin film is 1.0×10 -2 Ω•cm, the light transmittance of the film layer is 86%, and the electron mobility is 17 cm² / V·s.

[0032] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is as follows: in S13, the low-temperature stage, the medium-temperature stage, the high-temperature stage, and the cooling stage are all carried out in an air atmosphere, and the annealing stage is carried out in an inert atmosphere.

[0033] The relative density of the obtained titanium-based ceramic target is 98.2%, the grain size is 8.5 μm, and the resistivity is 6.5×10 -4 Ω•cm. The resistivity of the obtained titanium oxide thin film is 9.5×10 -4 Ω•cm, the light transmittance of the film layer is 82%, and the electron mobility is 20 cm² / V·s; the resistivity of the obtained ITO thin film is 1.5×10 -4 Ω•cm, the light transmittance of the film layer is 91%, and the electron mobility is 35 cm² / V·s; the resistivity of the obtained laminated thin film is 8.6×10 -4 Ω•cm, the light transmittance of the film layer is 84%, and the electron mobility is 25 cm² / V·s.

[0034] Through comparative analysis of Examples 1-3 and Comparative Examples 1-3, it can be seen that the ceramic target prepared by the method of the present invention has a lower resistivity, a higher average transmittance, and a higher electron mobility. The laminated thin film prepared by the method of the present invention has a lower resistivity, a higher average transmittance, and a higher electron mobility.

[0035] The above are only the preferred embodiments of the present invention, and do not impose any form of limitation on the present invention. Any equivalent transformation or modification made according to the essence of the present invention should be covered within the protection scope of the present invention.

Claims

1. A titanium-based ceramic target, characterized in that: In terms of mass fraction, the titanium-based ceramic target includes 96.4~98.3wt% of titanium oxide and 1.7~3.6% of doped oxide, wherein the doped oxide contains components and the mass fraction of each component is: 0.8~1.5wt% of niobium oxide, 0.5~1.0wt% of tantalum oxide, 0.3~0.8wt% of tungsten oxide, and 0.1~0.3wt% of aluminum oxide.

2. A method for preparing a titanium-based ceramic target, characterized in that: The main steps are as follows: Step 1: dispersing titanium oxide powder and doped oxide powder in a high-speed disperser to obtain a mixture, and then preparing the mixture, ultrapure water, a dispersant and a binder into a water-based slurry, and fully ball-milling; Step 2: spray drying the water-based slurry to obtain a powder; and then pressing the powder into a green compact; Step 3: Perform pressureless sintering in the following stages: (1) Low temperature stage: In an air atmosphere or an oxygen-nitrogen mixed atmosphere with an oxygen content of 15-25%, the temperature was first increased from room temperature to 300°C at a heating rate of 0.5°C / min, then increased to 550°C at a heating rate of 0.1°C / min, then increased to 750°C at a heating rate of 0.05°C / min, and kept at 750°C for 6 h, and finally increased to 1000°C at a heating rate of 0.5°C / min; (2) Medium temperature stage: In an oxygen-nitrogen mixed atmosphere with an oxygen content of 40-60%, first keep the temperature at 1000°C for 5 h, and then increase the temperature to 1350-1430°C at a heating rate of 0.5°C / min; (3) High temperature stage: keep at 1350-1430℃ for 9-20h, divided into three stages according to the holding time, each stage is maintained for 2-7h. The first and third stages are carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 40-60%, while the second stage is carried out in an oxygen-nitrogen mixed atmosphere with an oxygen content of 15-25%; (4) Cooling stage: In a pure oxygen atmosphere, first cool down to 1000°C at a cooling rate of 0.5°C / min, and then cool down to 800°C at a cooling rate of 0.3°C / min; (5) Annealing stage: in an inert atmosphere, first keep the temperature at 800 °C for 1-2 h, then cool to 600 °C at a cooling rate of 1 °C / min, keep the temperature at 600 °C for 1-2 h, and then cool to room temperature with the furnace to obtain a titanium-based ceramic target.

3. The method for preparing a titanium-based ceramic target according to claim 2, characterized in that: In step 1, the amount of ultrapure water added is 50-60wt% of the slurry solid content, the amount of dispersant added is 1.0-1.5wt% of the total mass of the mixture, and the amount of binder added is 1.5-2.5wt% of the total mass of the mixture.

4. The method for preparing a titanium-based ceramic target according to claim 2, characterized in that: In step 1, the dispersant is one or more of polycarboxylates, ammonium polyacrylates, citrates, polyvinyl pyrrolidone, and hexadecyltrimethylammonium bromide.

5. The method for preparing a titanium-based ceramic target according to claim 2, characterized in that: In step 1, the binder is one or more of polyvinyl alcohol, polyethylene glycol-1000, polymethacrylic acid, and carboxymethyl cellulose.

6. The method for preparing a titanium-based ceramic target according to claim 2, characterized in that: In step 1, the D50 of the titanium oxide powder is 0.8 μm, and the particle size of the doped oxide powder is not greater than 200 nm.

7. The method for preparing a titanium-based ceramic target according to claim 2, characterized in that: In step 2, the powder is placed in a mold, first dry pressed at a pressure of 80 MPa, and then cold isostatically pressed at a pressure of 300 MPa, and the density of the obtained green body is greater than 60%.

8. Application of a laminated film prepared from titanium-based ceramic target in silicon-based and perovskite solar cells.

9. The use according to claim 8, characterized in that: The laminated film is composited by a titanium-based film and an ITO film deposited on the surface of the titanium-based film, wherein the titanium-based film is obtained by sputtering a titanium-based ceramic target material, and the ITO film is obtained by sputtering an ITO target material.

10. The use according to claim 8, characterized in that: The substrate was placed on the base of a sputtering coater, and a titanium-based thin film with a thickness of 50 nm was first deposited by DC sputtering using a titanium-based ceramic target at a base temperature of 180°C; then an ITO thin film with a thickness of 50 nm was deposited by RF sputtering using an ITO target at a base temperature of 200°C.

Citation Information

Cited By

  • Titanium zirconium oxide composite target as well as preparation method and application thereof

    CN120965318A

  • A titanium dioxide-zirconium composite target, its preparation method and application

    CN120965318B