High-entropy relaxor ferroelectric polymer for dielectric energy storage and preparation method of high-entropy relaxor ferroelectric polymer

The treatment of relaxed ferroelectric polymers through proton beam irradiation induced high entropy super-simultaneous phase, which solved the problems of low charge and discharge efficiency and insufficient discharge energy density when used in energy storage capacitors, and achieved efficient energy storage performance and low loss.

CN120230314APending Publication Date: 2025-07-01HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510392128.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-31
Publication Date
2025-07-01

AI Technical Summary

Technical Problem

When used in energy storage capacitors, the existing relaxation ferroelectric polymers have low charge and discharge efficiency, insufficient discharge energy density, and high conductivity loss at high fields, which limits its application potential.

Method used

The high-entropy relaxed ferroelectric polymer with quasi-homotype phase boundary components is treated by proton beam irradiation, high-entropy super-schematic phase is induced, ferroelectric loss is reduced, dielectric constant and electrodepositing, and polarization saturation is delayed, and a high-entropy relaxed ferroelectric polymer film is prepared.

Benefits of technology

The discharge energy density and charge and discharge efficiency at low field are significantly improved, polarization saturation is delayed, conductive loss at high field is reduced, and high-performance dielectric energy storage materials are obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120230314A_ABST
    Figure CN120230314A_ABST
Patent Text Reader

Abstract

The invention belongs to the related technical field of dielectric energy storage materials, and discloses a high-entropy relaxor ferroelectric polymer for dielectric energy storage and a preparation method thereof, and the preparation method comprises the following steps: (1) dissolving a relaxor ferroelectric polymer with a morphotropic phase boundary component in an organic solvent to obtain a polymer solution; (2) casting the polymer solution on a glass substrate, heating to volatilize the solvent, and then heating and annealing in a vacuum environment to obtain a polymer film; (3) the polymer film is subjected to proton beam irradiation treatment, the dose of proton beam irradiation is 10 Mrad to 40 Mrad, the high-entropy superparaelectric phase is induced through the proton beam irradiation treatment, and the high-entropy relaxor ferroelectric polymer film for dielectric energy storage can be obtained. The high-entropy relaxor ferroelectric polymer for dielectric energy storage with high discharge energy density and high charge-discharge efficiency can be obtained, the bottleneck problem of hindering application of the relaxor ferroelectric polymer in an energy storage capacitor is solved, and a new scheme is provided for large-scale application of the relaxor ferroelectric polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to dielectric energy storage materials, and more specifically, relates to a high-entropy relaxor ferroelectric polymer for dielectric energy storage and a preparation method thereof. Background Art

[0002] Dielectric capacitors have an ultra-high power density and are key energy storage devices in modern electronic and electrical equipment. Compared with ceramics, polymer dielectric materials have the advantages of low cost and high breakdown strength. In particular, polyvinylidene fluoride (PVDF)-based ferroelectric polymers are ideal materials for developing high-energy density capacitors because of their high dielectric constant (more than 5 times that of commercial biaxially oriented polypropylene (BOPP)), and have attracted extensive attention in the academic and industrial fields. Among many PVDF-based polymers, relaxor ferroelectric polymers obtained by methods such as molecular copolymerization and electron beam irradiation have a low remanent polarization and can obtain a relatively high discharge energy density (>10 J / cm 3 ), and are considered to be the most promising ferroelectric polymers for dielectric energy storage. However, relaxor ferroelectric polymers have relatively high ferroelectric and leakage losses, resulting in a charge-discharge efficiency of only about 70%, far lower than that of commercial BOPP (still reaching 90% at 500 MV / m - 600 MV / m); in addition, relaxor ferroelectric polymers usually reach polarization saturation prematurely at an electric field strength far lower than the breakdown field strength, and the conduction loss dominates at high fields (electric field strength > 400 MV / m), which severely limits their ability to obtain a high discharge energy density. For this reason, researchers have proposed various methods, including defect modification of the molecular chain structure, blending of different polymers, and introduction of inorganic filler composites. Although these methods can improve the discharge energy density, the charge-discharge efficiency has not been effectively improved. Therefore, there is an urgent need to synergistically improve the discharge energy density and the charge-discharge efficiency to provide a new solution to the bottleneck problem of the energy storage application of high-dielectric-constant relaxor ferroelectric polymers. Summary of the Invention

[0003] Aiming at the above defects or improvement requirements of the prior art, the purpose of the present invention is to provide a high-entropy relaxor ferroelectric polymer for dielectric energy storage and a preparation method thereof. By using proton beam irradiation to treat a relaxor ferroelectric polymer with a quasi-homogeneous phase boundary composition, and controlling the dose of proton beam irradiation to be 10 Mrad - 40 Mrad, a high-entropy super paraelectric phase is induced in the relaxor ferroelectric polymer, which can reduce the ferroelectric loss at low electric fields (such as an electric field strength of 100 MV / m), increase the low-field dielectric constant and the high-field (electric field strength > 400 MV / m) polarization, delay the premature saturation of polarization, and obtain a high-entropy relaxor ferroelectric polymer for dielectric energy storage with a high discharge energy density and a high charge-discharge efficiency, solving the bottleneck problem that hinders the application of relaxor ferroelectric polymers in energy storage capacitors and providing a new solution for their large-scale application.

[0004] To achieve the above object, according to one aspect of the present invention, a method for preparing a high-entropy relaxor ferroelectric polymer for dielectric energy storage is provided, including the following steps:

[0005] (1) Dissolve a relaxor ferroelectric polymer with a morphotropic phase boundary composition in an organic solvent to obtain a polymer solution;

[0006] (2) Cast the polymer solution on a glass substrate, heat to volatilize the solvent, and then heat and anneal in a vacuum environment to obtain a polymer thin film;

[0007] (3) Perform proton beam irradiation treatment on the polymer thin film, and the dose of proton beam irradiation is 10 Mrad to 40 Mrad. In this way, a high-entropy super paraelectric phase is induced by proton beam irradiation treatment, and a high-entropy relaxor ferroelectric polymer thin film for dielectric energy storage can be obtained.

[0008] As a further preference of the present invention, the preparation method further includes the following steps:

[0009] (4) Use the high-entropy relaxor ferroelectric polymer thin film obtained in step (3) as an intermediate layer, and tightly attach insulating dielectric thin films on the upper and lower surfaces respectively as the upper layer and the lower layer to obtain a high-entropy relaxor ferroelectric polymer thin film for dielectric energy storage with a sandwich structure of upper layer - intermediate layer - lower layer.

[0010] As a further preference of the present invention, in step (1), the relaxor ferroelectric polymer with a morphotropic phase boundary composition is poly(vinylidene fluoride - trifluoroethylene - chlorotrifluoroethylene), and the molar ratio of vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene in the poly(vinylidene fluoride - trifluoroethylene - chlorotrifluoroethylene) is 65:31:4. The organic solvent is any one of N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone. The concentration of the polymer solution is 10 mg / mL to 100 mg / mL, the stirring time used is 8 h to 12 h, and the temperature is 15°C to 70°C.

[0011] As a further preference of the present invention, in step (2), the heating to volatilize the solvent and the heating and annealing in a vacuum environment are carried out in different heating furnaces; wherein, the heating to volatilize the solvent is carried out in a first heating furnace at 60°C to 70°C for 8 h to 12 h, and then cooled to room temperature with the furnace; the heating and annealing in a vacuum environment is specifically carried out in a second heating furnace. First, the temperature is raised to 60°C to 70°C, held for 8 h to 12 h, then the temperature is further raised to 105°C to 110°C, held for 12 h to 16 h, and then cooled to room temperature with the furnace;

[0012] Alternatively, the heating and volatilizing of the solvent and the heating and annealing in a vacuum environment are carried out in the same heating furnace. First, the heating furnace is heated to 60°C to 70°C and held for 8 h to 12 h to heat and volatilize the solvent, then the furnace temperature is maintained at 60°C to 70°C and vacuum pumping is started. In the vacuum environment, it is first held at 60°C to 70°C for 8 h to 12 h, then heated to 105°C to 110°C in the vacuum environment and held for 12 h to 16 h, and then cooled to room temperature with the furnace.

[0013] As a further preference of the present invention, in step (3), the dose of the proton beam irradiation is 20 Mrad;

[0014] Preferably, the energy of the proton beam irradiation is 20 MeV, and the proton beam is incident perpendicular to the surface of the thin film.

[0015] As a further preference of the present invention, in step (4), the insulating dielectric thin film is made of an inorganic dielectric material or an organic dielectric material. Among them, the inorganic dielectric material is preferably any one of SiO2 and Al2O3, and the organic dielectric material is preferably any one of polyetherimide, polyimide, and polymethyl methacrylate;

[0016] The tight fitting is achieved by plating and / or hot pressing.

[0017] As a further preference of the present invention, the insulating dielectric thin film is a polyetherimide thin film, and the tight fitting is achieved by hot pressing.

[0018] As a further preference of the present invention, in step (1), the relaxor ferroelectric polymer with a morphotropic phase boundary component is poly(vinylidene fluoride-trifluoroethylene-trichlorofluoroethylene), and the molar ratio of vinylidene fluoride, trifluoroethylene, and trichlorofluoroethylene in the poly(vinylidene fluoride-trifluoroethylene-trichlorofluoroethylene) is 65:31:4;

[0019] The organic solvent is N,N-dimethylformamide;

[0020] The concentration of the polymer solution is 40 mg / ml.

[0021] According to another aspect of the present invention, the present invention provides a high-entropy relaxor ferroelectric polymer thin film for dielectric energy storage prepared by the above preparation method, or a high-entropy relaxor ferroelectric polymer thin film for dielectric energy storage having a sandwich structure of upper layer - middle layer - lower layer prepared by the above preparation method.

[0022] According to still another aspect of the present invention, the present invention provides a dielectric energy storage device, including the above high-entropy relaxor ferroelectric polymer thin film for dielectric energy storage or a high-entropy relaxor ferroelectric polymer thin film for dielectric energy storage having a sandwich structure of upper layer - middle layer - lower layer.

[0023] Through the above technical solution conceived by the present invention, compared with the prior art, the method of the present invention utilizes proton beam irradiation, and by controlling the dose of proton beam irradiation to be 10 Mrad to 40 Mrad, a high-entropy super paraelectric phase is induced in the relaxor ferroelectric polymer, significantly reducing the ferroelectric loss at low electric fields (electric field strength of 100 MV / m), and increasing the low-field dielectric constant and high-field (electric field strength > 400 MV / m) polarization, delaying the premature saturation of polarization, and a high-entropy relaxor ferroelectric polymer for dielectric energy storage with high discharge energy density and high charge-discharge efficiency can be obtained. Taking the product of Example 2 hereinafter as an example, a discharge energy density of 3.2 J / cm³ can be obtained only at an ultra-low electric field strength of 100 MV / m 3 The charge-discharge efficiency is 87%, far exceeding the performance of existing polymer dielectric materials at low fields (for example, the discharge energy density of BOPP at 100 MV / m is only 0.1 J / cm³ 3 , and the discharge energy density of the original relaxor ferroelectric polymer in Comparative Example 1 hereinafter at 100 MV / m is only 1.2 J / cm³ 3 ). In particular, the present invention can further construct a sandwich structure with the prepared high-entropy relaxor ferroelectric polymer for dielectric energy storage as the intermediate layer, which can more effectively suppress the high-field (electric field strength > 400 MV / m) conduction loss. Taking Example 4 hereinafter as an example, a discharge energy density of 23.1 J / cm³ can be obtained at 600 MV / m 3 The charge-discharge efficiency > 90%.

[0024] Specifically, the present invention can achieve the following beneficial effects:

[0025] 1. The present invention utilizes proton beam irradiation to induce the formation of a high-entropy super paraelectric phase in the relaxor ferroelectric polymer, reducing the ferroelectric loss at low electric fields, delaying the appearance of polarization saturation, obtaining a higher maximum polarization intensity, and achieving high energy density and high charge-discharge efficiency at low fields (electric field strength of 100 MV / m). Taking Example 2 hereinafter as an example, the dielectric constant of the poly(vinylidene fluoride-trifluoroethylene-trichlorofluoroethylene) (molar content ratio of 65 / 31 / 4) polymer after 20 Mrad proton beam irradiation is increased to 75.4 at a frequency of 1 kHz, and the discharge energy density at a field strength of 100 MV / m is 3.2 J / cm³ 3 , the charge-discharge efficiency is 87.2%, approaching the discharge energy density and charge-discharge efficiency of commercial BOPP at high electric fields of 500 MV / m to 600 MV / m; the discharge energy density at a high electric field of 700 MV / m is 45.8 J / cm³ 3 , and the charge-discharge efficiency is 63.8%, far higher than the discharge energy density of existing polymers at the same electric field (for example, the discharge energy density of polyetherimide at 700 MV / m is about 8 J / cm³ 3 ).

[0026] Before the irradiation treatment of the present invention, the relaxor ferroelectric polymer needs to be a relaxor ferroelectric polymer with a morphotropic phase boundary composition, so that a high-entropy super paraelectric phase can be induced to form in the relaxor ferroelectric polymer by irradiating with a proton beam with an irradiation dose of 10 Mrad to 40 Mrad. At the same time, common particle beam irradiation methods include proton beam irradiation, electron beam irradiation, etc. The present invention needs to use proton beam irradiation and strictly control the irradiation dose of the proton beam to 10 Mrad to 40 Mrad. If electron beam irradiation is used, even if the irradiation dose meets 10 Mrad to 40 Mrad, the effect of inducing the formation of a high-entropy super paraelectric phase cannot be achieved (as exemplified in Comparative Examples 7 to 9 hereinafter).

[0027] 2. On the basis of inducing the formation of a high-entropy super paraelectric phase by using proton beam irradiation, the present invention further utilizes a sandwich structure to suppress the conductive loss caused by electron injection at the interface between the high-entropy polymer and the electrode under a high field (electric field strength > 400 MV / m), significantly improving the discharge efficiency and obtaining an ultra-high discharge energy density. Taking Example 4 hereinafter as an example (Example 4 is based on Example 2, using the film prepared in Example 2 as the intermediate layer, and further forming a high-entropy relaxor ferroelectric polymer film for dielectric energy storage with a sandwich structure of upper layer - intermediate layer - lower layer), the discharge energy density of the all-organic sandwich structure film based on the high-entropy relaxor ferroelectric polymer is 23.1 J / cm 3 at a field strength of 600 MV / m, and the charge-discharge efficiency is greater than 90%, exceeding the energy storage performance of existing polymer-based dielectric energy storage materials, and solving the problems of high conductive loss and low charge-discharge efficiency of current relaxor ferroelectric polymers under high fields.

[0028] 3. The preparation method of the present invention only uses proton beam irradiation to modify the relaxor ferroelectric polymer and the lamination of different film layers, without complex physical blending or chemical synthesis operations, and the process is simple, suitable for large-scale processing and preparation.

[0029] 4. The high-entropy relaxor ferroelectric polymer prepared by the present invention has the characteristics of high energy storage density and high charge-discharge efficiency, can be used to manufacture dielectric energy storage devices, and can meet the application requirements of fast charge and discharge in the new energy field, such as new energy vehicles, electromagnetic energy equipment, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a schematic flow chart of a preparation method of a high-entropy relaxor ferroelectric polymer for dielectric energy storage provided by the present invention.

[0031] Figure 2 is a relationship diagram of the dielectric constant and the irradiation dose (i.e., Examples 1 to 3 and Comparative Examples 1 to 2) of the high-entropy relaxor ferroelectric polymer provided by the present invention at a frequency of 1 kHz.

[0032] Figure 3It is a comparison chart of the discharge energy density and charge-discharge efficiency of the high-entropy relaxor ferroelectric polymer obtained in Example 2 of the present invention, the products of Comparative Example 1, Comparative Example 3, and Comparative Example 4 under an electric field of 100 MV / m, and commercial BOPP under electric fields of 500 MV / m and 600 MV / m; wherein, Figure 3 a in Figure 3 corresponds to the discharge energy density,

[0033] Figure 4 It is a comparison chart of the discharge energy density and charge-discharge efficiency of the products of Example 2, Example 4 of the present invention, and Comparative Example 1, Comparative Example 4 under different electric fields.

[0034] Figure 5 It is a comparison chart of the discharge energy density and charge-discharge efficiency of the product of Example 4 of the present invention and commercial BOPP under different electric fields.

[0035] Figure 6 It is the temperature-irradiation dose phase diagram of the high-entropy relaxor ferroelectric polymer provided by the present invention (different irradiation doses correspond to Examples 1 to 3 and Comparative Examples 1 to 2 respectively).

[0036] Figure 7 It is the infrared spectrogram of the products of Comparative Examples 1-2 and Examples 1-3 at different wavenumbers; wherein, Figure 7 a in -1 corresponds to the wavenumber range of 1470 cm -1 to Figure 7 1950 cm, -1 b in -1 corresponds to the wavenumber range of 3160 cm

[0037] Figure 8 It is a relationship diagram of the polarization intensity and electric field intensity of the products of Comparative Example 1 and Example 2 at a frequency of 1 kHz; wherein, Figure 8 a in Figure 8 corresponds to the product of Comparative Example 1,

[0038] Figure 9 b in

[0039] Figure 10 corresponds to the product of Example 2. Figure 10 a in Figure 10 corresponds to the samples of Comparative Example 4 and Comparative Example 5, Detailed implementation manners

[0040] In order to make the objectives, technical solutions and advantages of the present invention clearer and more understandable, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. In addition, the technical features involved in the various implementation manners of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0041] The preparation method of the high-entropy relaxor ferroelectric polymer for dielectric energy storage in the present invention may include the following steps:

[0042] Step 1, dissolving a relaxor ferroelectric polymer with a morphotropic phase boundary composition in an organic solvent to obtain a polymer solution.

[0043] For example, the relaxor ferroelectric polymer with a morphotropic phase boundary composition may be poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene) (P(VDF-TrFE-CTFE)), with a molar content ratio of 65 / 31 / 4 (65 / 31 / 4 mol%), the organic solvent may be any one of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP), the concentration of the polymer solution may be 10 mg / mL to 100 mg / mL, the stirring time used may be 8 h to 12 h, and the temperature may be 15°C to 70°C.

[0044] P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) used in the subsequent examples was commercially purchased and itself has a morphotropic phase boundary composition;

[0045] P(VDF-TrFE-CTFE) (65.6 / 26.7 / 7.7 mol%) and P(VDF-TrFE-CTFE) (65.4 / 26.2 / 8.4 mol%) used in the subsequent comparative examples were also commercially purchased, but due to the too high content of CTFE, these two materials do not have a morphotropic phase boundary composition by themselves. P(VDF-HFP) (85 / 15 wt%) used does not have a morphotropic phase boundary composition by itself and was also commercially purchased.

[0046] Step 2, casting the polymer solution on a glass substrate, heating to volatilize the solvent, and then heating and annealing in a vacuum environment to obtain a polymer thin film.

[0047] Among them, the two processes of heating and volatilizing the solvent and annealing by heating in a vacuum environment can be completed either in the same heating furnace with a vacuum pumping function or in different heating furnaces. Taking the case of being completed in different heating furnaces (the subsequent examples use different heating furnaces), the process of heating and volatilizing the solvent can be: heating to 60°C to 70°C, holding for 8h to 12h, and cooling to room temperature with the furnace.

[0048] The process of annealing by heating in a vacuum environment can be: heating to 60°C to 70°C, holding for 8h to 12h, then heating to 105°C to 110°C, holding for 12h to 16h, and cooling to room temperature with the furnace.

[0049] If the two processes of heating and volatilizing the solvent and annealing by heating in a vacuum environment use the same heating furnace, after the process of heating and volatilizing the solvent is completed, instead of cooling, vacuum pumping can be started under the temperature condition of maintaining 60°C to 70°C, and directly carry out the process of annealing by heating in a vacuum environment, that is, in a vacuum environment, first heat to 60°C to 70°C, hold for 8h to 12h, then heat to 105°C to 110°C, hold for 12h to 16h, and cool to room temperature with the furnace.

[0050] Step 3: Perform proton beam irradiation on the polymer film to induce a high-entropy super paraelectric phase, and obtain a high-entropy relaxor ferroelectric polymer film.

[0051] Among them, the energy of the proton beam irradiation can be, for example, 20 MeV, the flux can be 2×10 8 p / (cm 2 ·s), the spot size can be 1×1 cm 2 , the direction is perpendicular to the film surface, and the dose can be 10 Mrad to 40 Mrad.

[0052] Step 4: Use the high-entropy relaxor ferroelectric polymer film as the middle layer, and tightly attach an insulating dielectric film on each of the upper and lower surfaces as the upper and lower layers to obtain a sandwich structure with upper, middle, and lower three-layer structures.

[0053] Specifically, the optional materials of the insulating dielectric film include, for example, inorganic dielectric materials such as SiO2, Al2O3, etc., and any one of polymer organic dielectric materials such as polyetherimide, polyimide, polymethyl methacrylate, etc. The bonding method includes any one of plating and hot pressing.

[0054] The following are specific examples:

[0055] Example 1

[0056] The preparation method of the high-entropy relaxor ferroelectric polymer for dielectric energy storage provided by Example 1 of the present invention mainly includes the following steps:

[0057] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 10 Mrad.

[0058] Example 2

[0059] The preparation method of the high-entropy relaxor ferroelectric polymer for dielectric energy storage provided in Example 2 of the present invention mainly includes the following steps:

[0060] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 20 Mrad.

[0061] Example 3

[0062] The preparation method of the high-entropy relaxor ferroelectric polymer for dielectric energy storage provided in Example 3 of the present invention mainly includes the following steps:

[0063] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 40 Mrad.

[0064] Example 4

[0065] The preparation method of the high-entropy relaxor ferroelectric polymer for dielectric energy storage provided in Example 4 of the present invention mainly includes the following steps:

[0066] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and then cooled to room temperature in the furnace. Then, it was irradiated with a proton beam at a dose of 20 Mrad. Finally, using polyetherimide films as the upper and lower surface layers, a sandwich-structured film was tightly laminated by a hot pressing method.

[0067] Example 5

[0068] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 60 °C for 8 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 60 °C in a vacuum environment and kept for 8 h, then further heated to 110 °C and kept for 12 h, and then cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 10 Mrad.

[0069] Comparative Example 1

[0070] The preparation method of the relaxor ferroelectric polymer for dielectric energy storage provided in Comparative Example 1 mainly includes the following steps:

[0071] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and then cooled to room temperature in the furnace. No proton beam irradiation treatment was carried out.

[0072] Comparative Example 2

[0073] The preparation method of the relaxor ferroelectric polymer for dielectric energy storage provided in Comparative Example 2 mainly includes the following steps:

[0074] 0.4 g of P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 5 Mrad.

[0075] Comparative Example 3

[0076] The preparation method of the relaxor ferroelectric polymer for dielectric energy storage provided by Comparative Example 3 mainly includes the following steps:

[0077] 0.4 g of P(VDF-TrFE-CTFE) (65.6 / 26.7 / 7.7 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. No proton beam irradiation treatment was carried out.

[0078] Comparative Example 4

[0079] The preparation method of the relaxor ferroelectric polymer for dielectric energy storage provided by Comparative Example 4 mainly includes the following steps:

[0080] 0.4 g of P(VDF-TrFE-CTFE) (65.4 / 26.2 / 8.4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface and kept at 70 °C for 12 h, then cooled to room temperature in the furnace. Subsequently, it was heated to 70 °C in a vacuum environment and kept for 12 h, then further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. No proton beam irradiation treatment was carried out.

[0081] Comparative Example 5

[0082] The preparation method of the relaxor ferroelectric polymer for dielectric energy storage provided by Comparative Example 5 mainly includes the following steps:

[0083] 0.4 g of P(VDF-TrFE-CTFE) (65.4 / 26.2 / 8.4 mol%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface, kept at 70 °C for 12 h, cooled to room temperature in the furnace, then heated to 70 °C in a vacuum environment and kept for 12 h, further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 20 Mrad.

[0084] Comparative Example 6

[0085] The preparation method of the relaxor ferroelectric polymer for dielectric energy storage provided by Comparative Example 6 mainly includes the following steps:

[0086] 0.4 g of P(VDF-HFP) (85 / 15 wt%) was added to 10 mL of DMF solution to prepare a polymer solution with a concentration of 40 mg / mL. The solution was stirred at a rate of 500 rpm / min at 25 °C for 12 h. After thorough mixing, the solution was cast on the glass surface, kept at 70 °C for 12 h, cooled to room temperature in the furnace, then heated to 70 °C in a vacuum environment and kept for 12 h, further heated to 105 °C and kept for 16 h, and finally cooled to room temperature in the furnace. Finally, it was irradiated with a proton beam at a dose of 20 Mrad.

[0087] Comparative Example 7

[0088] This comparative example is generally the same as Example 1, except that: instead of using proton beam irradiation, electron beam irradiation with a dose of 10 Mrad was used.

[0089] Comparative Example 8

[0090] This comparative example is generally the same as Example 2, except that: instead of using proton beam irradiation, electron beam irradiation with a dose of 20 Mrad was used.

[0091] Comparative Example 9

[0092] This comparative example is generally the same as Example 3, except that: instead of using proton beam irradiation, electron beam irradiation with a dose of 40 Mrad was used.

[0093] The dielectric energy storage performance of the products obtained in Comparative Examples 7 to 9 at low fields of 100 MV / m and high fields of >400 MV / m is at the same level as that of Comparative Examples 1, 3, and 4, with almost no improvement.

[0094] Table 1. Comparison of dielectric energy storage performance of the products of Examples 1-5 and Comparative Examples 1-4 with commercial BOPP materials at 100 MV / m

[0095]

[0096] The discharge energy density and charge-discharge efficiency of the products of Example 2, Example 4, Comparative Example 1, and Comparative Example 4 under other electric fields in the range of 50 - 700 MV / m are as follows Figure 4 shown. It is not difficult to see from this that the discharge energy density of the product of Example 2 is the best, and the charge-discharge efficiency of the product of Example 4 is the best. The discharge energy density of the product of Example 2 is 45.8 J / cm 3 under an electric field of 700 MV / m, and the charge-discharge efficiency is 63.8%, which is much higher than the discharge energy density of existing polymers under the same electric field.

[0097] At the same time, it can be seen from Figure 5 that the charge-discharge efficiency of the product of Example 4 is basically the same as that of commercial BOPP in the range of 50 MV / m - 500 MV / m, but the discharge energy density of the product of Example 4 is better than that of commercial BOPP.

[0098] In addition, infrared spectroscopy was performed on Comparative Examples 1 - 2 and Examples 1 - 3 respectively, and the results are as follows Figure 7 shown. It is not difficult to see from this that for the products of Comparative Example 2 and Examples 1 - 3 obtained through irradiation treatment, compared with the product of Comparative Example 1 without irradiation, peaks of C=O, C=C, and -OH appear. This indicates that these structures are formed during the irradiation process, and the entropy of the material shows an increasing trend; moreover, the greater the irradiation dose, the more the contents of these structures of C=O, C=C, and -OH, and the greater the entropy increase.

[0099] Figure 8 Shown is the relationship diagram of the polarization intensity and the electric field strength of Comparative Example 1 and Example 2 Figure 9 Shown is the relationship diagram of the polarization intensity and the electric field strength of Comparative Example 1 and Example 2 at 100 MV / m. It can be seen from this that at all electric fields, the polarization intensity of Example 2 is significantly higher than that of Comparative Example 1, indicating that the polarization of the high-entropy relaxor ferroelectric polymer is higher; at the same time, the curve of Comparative Example 1 begins to tend to be horizontal at the end when the electric field is 200 MV / m, while that of Example 2 only slowly appears after exceeding 300 MV / m, indicating that the high-entropy relaxor ferroelectric polymer delays the saturation of polarization.

[0100] From Figure 10 it can be seen that the relationship between the polarization intensity and the electric field strength of two polymers without the morphotropic phase boundary component does not change significantly after proton beam irradiation. Compared with the significant changes in Figure 8 , Figure 9 , it can be seen that polymers without the morphotropic phase boundary component cannot achieve the high-entropy super paraelectric phase through proton beam irradiation.

[0101] The above embodiments are only examples. For example, for relaxor ferroelectric polymers with a morphotropic phase boundary composition, in addition to P(VDF-TrFE-CTFE) (65 / 31 / 4 mol%), other relaxor ferroelectric polymers with a morphotropic phase boundary composition can also be used.

[0102] It is easy for those skilled in the art to understand that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent replacements, and improvements made within the spirit and principle of the present invention shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage, characterized in that: The following steps are involved: (1) dissolving a relaxor ferroelectric polymer having a morphotropic phase boundary component in an organic solvent to obtain a polymer solution; (2) casting the polymer solution on a glass substrate, heating to volatilize the solvent, and then heating and annealing in a vacuum environment to obtain a polymer film; (3) The polymer film is subjected to proton beam irradiation treatment, and the proton beam irradiation dose is 10 Mrad to 40 Mrad. In this way, a high entropy superparaelectric phase is induced by proton beam irradiation treatment, and a high entropy relaxor ferroelectric polymer film for dielectric energy storage can be obtained.

2. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 1, characterized in that: The following steps are also included: (4) The high entropy relaxor ferroelectric polymer film for dielectric energy storage obtained in step (3) is used as an intermediate layer, and insulating dielectric films are tightly attached to the upper and lower surfaces as the upper and lower layers respectively, to obtain a high entropy relaxor ferroelectric polymer film for dielectric energy storage having a sandwich structure of upper layer-intermediate layer-lower layer stacking.

3. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 1 or 2, characterized in that: In step (1), the relaxor ferroelectric polymer having a quasi-isotropic phase boundary component is polyvinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene, the molar ratio of vinylidene fluoride, trifluoroethylene and chlorotrifluoroethylene in the polyvinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene is 65:31:4, the organic solvent is any one of N,N-dimethylformamide, dimethyl sulfoxide and N-methylpyrrolidone, the concentration of the polymer solution is 10 mg / mL to 100 mg / mL, the stirring time is 8 h to 12 h, and the temperature is 15°C to 70°C.

4. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 1 or 2, characterized in that: In step (2), the heating to volatilize the solvent and the heating annealing in a vacuum environment are performed in different heating furnaces; wherein the heating to volatilize the solvent is carried out in a first heating furnace at 60°C to 70°C for 8h to 12h, and then cooled to room temperature with the furnace; the heating annealing in a vacuum environment is specifically carried out in a second heating furnace, firstly heating to 60°C to 70°C, keeping warm for 8h to 12h, then heating to 105°C to 110°C, keeping warm for 12h to 16h, and then cooling to room temperature with the furnace; Alternatively, the heating to volatilize the solvent and the heating annealing in a vacuum environment are carried out in the same heating furnace, that is, the heating furnace is first heated to 60°C to 70°C and kept warm for 8h to 12h to heat and volatilize the solvent, and then the furnace temperature is maintained at 60°C to 70°C to start vacuuming, and the temperature is kept at 60°C to 70°C for 8h to 12h in a vacuum environment, and then the temperature is raised to 105°C to 110°C in a vacuum environment and kept warm for 12h to 16h, and then the furnace is cooled to room temperature.

5. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 1 or 2, characterized in that: In step (3), the dose of the proton beam irradiation is 20 Mrad; Preferably, the energy of the proton beam irradiation is 20 MeV, and the proton beam is incident perpendicularly to the surface of the film.

6. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 2, characterized in that: In step (4), the insulating dielectric film is made of an inorganic dielectric material or an organic dielectric material, wherein the inorganic dielectric material is preferably any one of SiO2 and Al2O3, and the organic dielectric material is preferably any one of polyetherimide, polyimide, and polymethyl methacrylate; The close fit is achieved by plating and / or hot pressing.

7. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 2, characterized in that: The insulating dielectric film is a polyetherimide film, and the close adhesion is achieved by hot pressing.

8. The method for preparing a high entropy relaxor ferroelectric polymer for dielectric energy storage according to claim 1 or 2, characterized in that: In step (1), the relaxor ferroelectric polymer having a quasi-isotropic phase boundary component is polyvinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene, and the molar ratio of vinylidene fluoride, trifluoroethylene and chlorotrifluoroethylene in the polyvinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene is 65:31:4; The organic solvent is N,N-dimethylformamide; The concentration of the polymer solution was 40 mg / ml.

9. A high entropy relaxor ferroelectric polymer film for dielectric energy storage prepared by the preparation method as described in any one of claims 1, 3, 4, 5, and 8, or a high entropy relaxor ferroelectric polymer film for dielectric energy storage having a sandwich structure of upper layer-middle layer-lower layer stacked by the preparation method as described in any one of claims 2-8.

10. A dielectric energy storage device, characterized in that: It comprises the high entropy relaxor ferroelectric polymer film for dielectric energy storage as claimed in claim 9 or a high entropy relaxor ferroelectric polymer film for dielectric energy storage having a sandwich structure of upper layer-middle layer-lower layer stacking.