Method for recovering valuable metals in waste lithium batteries and synchronously degrading antibiotics in water

By reacting the cathode material of waste lithium battery with oxidant, adjusting the pH value for solid-liquid separation, and using transition metal catalytic oxidant to generate free radicals, the problems of low leaching rate of valuable metals and low antibiotic degradation efficiency in lithium battery recycling are solved, and efficient recycling of valuable metals and synchronous degradation of antibiotics are achieved, with good economic and environmental benefits.

CN120441032APending Publication Date: 2025-08-08GUANGDONG INST OF ECO ENVIRONMENT & SOIL SCI

Patent Information

Application Number
CN202510565304.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-30
Publication Date
2025-08-08

AI Technical Summary

Technical Problem

The existing lithium battery recycling process has the problems of high environmental hazards of leaching solvents and slow leaching rate, and the existing antibiotic degradation methods are difficult to efficiently and synchronize the treatment of antibiotics in wastewater.

Method used

The positive electrode material of the used lithium battery is used to react with the oxidant, adjust the pH value for solid-liquid separation, and free radicals are generated by transition metal catalytic oxidant, precipitation and recovery of valuable metals and degradation of antibiotics.

Benefits of technology

It realizes efficient recycling of valuable metals and synchronous degradation of antibiotics, with simple operation, significant economic and environmental benefits, and is suitable for the treatment of various antibiotic categories.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005385764250000011
    Figure HDA0005385764250000011
  • Figure HDA0005385764250000012
    Figure HDA0005385764250000012
  • Figure HDA0005385764250000021
    Figure HDA0005385764250000021
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery recovery and wastewater treatment, and discloses a method for recovering valuable metals in waste lithium batteries and synchronously degrading antibiotics in water. The method comprises the following steps: adding a waste lithium battery positive electrode material and an oxidizing agent into antibiotic wastewater, and reacting to obtain a positive electrode metal leaching solution; adjusting the pH value of the anode metal leachate to 9-14, and carrying out solid-liquid separation to obtain a lithium-rich filtrate and a transition metal precipitate; and adding a precipitator into the lithium-rich filtrate, carrying out precipitation reaction, and collecting a lithium-rich precipitate. According to the method provided by the invention, based on an advanced oxidation process, the transition metal in the positive electrode material of the waste lithium battery can be oxidized and dissolved by an oxidizing agent to recover metal resources, and can also be used as a catalyst to activate the oxidizing agent to generate free radicals and degrade antibiotics, so that metal recovery and pollutant degradation are synchronously completed in a single system; the method is easy to operate, co-treatment of urban solid waste and wastewater is promoted, and good ecological environmental benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery recovery and wastewater treatment, and in particular to a method for recovering valuable metals in waste lithium batteries and simultaneously degrading antibiotics in water. Background Art

[0002] As lithium-ion batteries are used in large quantities, the production of used lithium batteries has also increased rapidly. Used lithium batteries are rich in metal resources such as lithium, nickel, cobalt, and manganese. If not properly disposed of, they will lead to environmental pollution and waste of resources. Therefore, recycling and comprehensive utilization of used lithium batteries are the only way to properly dispose of them.

[0003] Currently, the main recycling processes for used lithium batteries include pyrometallurgy, hydrometallurgy, and biometallurgy. Hydrometallurgy has become the mainstream method for recycling retired lithium batteries due to its low energy consumption and environmental friendliness. However, while hydrometallurgy has achieved good results in extracting key metal resources from retired lithium batteries, it still faces challenges such as significant environmental hazards posed by the leaching solvents and slow leaching rates.

[0004] Antibiotics are widely used in healthcare, aquaculture, and other fields. They have a strong ability to migrate in the environment and can be continuously released into the water environment through various pathways, posing a potential threat to aquatic organisms and ecosystems. Urban medical wastewater discharge is a major source of antibiotics in water bodies.

[0005] Currently, methods for removing antibiotics from typical urban medical wastewater include adsorption, membrane filtration, and advanced oxidation degradation. Advanced oxidation processes, through the interaction between materials and advanced oxidation reagents, can generate a variety of reactive oxygen species, breaking down organic pollutants such as antibiotics into carbon dioxide and water, making them an effective method for removing antibiotics from wastewater. Transition metals can act as effective activating components, activating advanced oxidation reagents such as potassium persulfate, hydrogen peroxide, and peracetic acid, causing them to decompose and produce free radicals, thereby rapidly degrading organic matter (such as antibiotics).

[0006] Therefore, developing an advanced oxidation process that uses transition metals in retired lithium batteries to activate advanced oxidation reagents and then degrade antibiotics is of great significance for achieving the recovery of valuable metals in retired lithium batteries and the simultaneous degradation of antibiotics. Summary of the Invention

[0007] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the present invention aims to provide a method for recovering valuable metals from waste lithium batteries and simultaneously degrading antibiotics.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] The present invention provides a method for recovering valuable metals in waste lithium batteries and simultaneously degrading antibiotics in water, comprising the following steps:

[0010] S1. Adding waste lithium battery positive electrode materials and an oxidant to antibiotic wastewater to react and obtain a positive electrode metal leachate;

[0011] S2, adjusting the pH of the positive electrode metal leachate to 9-14, and performing solid-liquid separation to obtain a lithium-rich filtrate and a transition metal precipitate;

[0012] S3. Adding a precipitant to the lithium-rich filtrate to undergo precipitation reaction, and collecting the lithium-rich precipitate.

[0013] In some embodiments of the present invention, in step S1, the antibiotic concentration in the antibiotic wastewater is 1-100 mg / L.

[0014] In some preferred embodiments of the present invention, in step S1, the antibiotic concentration in the antibiotic wastewater is 10-100 mg / L.

[0015] In some embodiments of the present invention, the antibiotics include at least one of tetracycline antibiotics, sulfonamide antibiotics, chloramphenicol antibiotics, and β-lactam antibiotics.

[0016] In some embodiments of the present invention, the tetracycline antibiotics include at least one of tetracycline and oxytetracycline.

[0017] In some embodiments of the present invention, the sulfonamide antibiotic includes at least one of sulfadiazine, sulfamethoxazole, and sulfacetamide.

[0018] In some embodiments of the present invention, the chloramphenicol antibiotic includes chloramphenicol.

[0019] In some embodiments of the present invention, the β-lactam antibiotic includes cephradine.

[0020] In some embodiments of the present invention, in step S1, the amount of the waste lithium battery positive electrode material added is 1-30 g / L.

[0021] In some preferred embodiments of the present invention, in step S1, the amount of the waste lithium battery positive electrode material added is 10-30 g / L.

[0022] In some embodiments of the present invention, in step S1, the cathode material of the waste lithium battery is selected from LiFePO4, LiCoO2, LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.33 Co 0.33 Mn 0.33 O2 or LiMn2O4.

[0023] In some embodiments of the present invention, the waste lithium battery positive electrode material is obtained by a method comprising the following steps:

[0024] The waste lithium battery is discharged, disassembled and stripped to obtain the waste lithium battery positive electrode material.

[0025] In some embodiments of the present invention, the discharging comprises placing the waste lithium battery in saturated salt water.

[0026] In some embodiments of the present invention, the stripping comprises dissolving the positive electrode binder using N-methylpyrrolidone.

[0027] In some embodiments of the present invention, the waste lithium battery is selected from lithium iron phosphate battery, lithium cobalt oxide battery, nickel cobalt lithium manganese oxide battery or lithium manganese oxide battery.

[0028] In some embodiments of the present invention, in step S1, the volume concentration of the oxidant is 10%-20%; the dosage of the oxidant is 5%-15% of the volume of the antibiotic wastewater.

[0029] In some preferred embodiments of the present invention, in step S1, the volume concentration of the oxidant is 10%-15%; the dosage of the oxidant is 10%-15% of the volume of the antibiotic wastewater.

[0030] In some embodiments of the present invention, the oxidant is selected from at least one of peroxyformic acid, peracetic acid, pervaleric acid, perbenzoic acid, and m-chloroperbenzoic acid.

[0031] In some preferred embodiments of the present invention, the oxidizing agent is peracetic acid.

[0032] In some embodiments of the present invention, in step S1, the reaction temperature is 10-90°C, the reaction time is 1-3 hours, and the system pH is 0.1-6.

[0033] In some preferred embodiments of the present invention, in step S1, the reaction temperature is 20-30°C, the reaction time is 1-2 hours, and the system pH is 4-6.

[0034] In some embodiments of the present invention, in step S2, the reagent used to adjust the pH of the positive electrode metal leachate is selected from at least one of sodium hydroxide and potassium hydroxide.

[0035] In some embodiments of the present invention, in step S3, the concentration of the precipitant is 3-7 mol / L; and the amount of the precipitant added is 10%-50% of the volume of the lithium-rich filtrate.

[0036] In some preferred embodiments of the present invention, in step S3, the concentration of the precipitant is 3-5 mol / L; and the amount of the precipitant added is 10%-30% of the volume of the lithium-rich filtrate.

[0037] In some embodiments of the present invention, in step S3, the precipitant comprises a sodium carbonate solution.

[0038] In some embodiments of the present invention, in step S3, the precipitation reaction temperature is 90-100° C. and the time is 5-15 hours.

[0039] In some preferred embodiments of the present invention, in step S3, the precipitation reaction temperature is 90-100° C. and the time is 6-12 h.

[0040] In some embodiments of the present invention, step S3 further includes the steps of washing and drying the lithium-rich precipitate.

[0041] In some embodiments of the present invention, the washing agent comprises 90-100°C hot water.

[0042] The basic principles of the present invention are described as follows:

[0043] Advanced oxidation processes (AOPs) are a process that generates strong oxidizing free radicals (such as OH, SO4 - The core of the technology is to use oxidants (such as persulfates, hydrogen peroxide, peroxyacids, etc.) to generate highly active free radicals under the action of catalysts (such as transition metals), thereby rapidly decomposing organic matter (such as antibiotics). In the present invention, the main reaction process between the cathode material of waste lithium batteries, oxidants, and antibiotics is as follows:

[0044] ① Catalytic oxidant decomposition: The transition metal in the cathode material of waste lithium batteries can activate the oxidant, causing it to decompose and produce free radicals. The generated free radicals can efficiently degrade organic matter;

[0045] ② Extraction of valuable metals in the positive electrode: the transition metals (such as Co 3+ 、Mn 4+ etc.) usually exist in a high valence state and are difficult to dissolve directly. They can be reduced to a low valence state (such as Co) through the redox reaction process of oxidants such as peroxyacids. 2+ 、Mn 2+etc.), thereby promoting metal leaching.

[0046] The method provided by the present invention recovers valuable metals in waste lithium batteries and simultaneously degrades antibiotics in water. The method is based on an advanced oxidation process and utilizes an oxidant to react with a positive electrode material of the waste lithium battery under acidic conditions (pH = 0.1-6) to dissolve transition metals therein and disintegrate the positive electrode structure. The dissolved transition metal ions can catalyze more oxidants to generate free radicals, thereby degrading antibiotics in the wastewater. By adjusting the pH of the positive electrode metal leachate to 9-14, the transition metal ions are separated by forming insoluble hydroxide precipitates, while the lithium ions remain in the solution. By adding a precipitant, a lithium-rich precipitate with low solubility is generated. The transition metal hydroxide precipitate and the lithium-rich precipitate are collected, thereby realizing the recovery of lithium and transition metals.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] 1) The method provided by the present invention for recovering valuable metals from waste lithium batteries and simultaneously degrading antibiotics in water is based on an advanced oxidation process. This process allows transition metals (such as Co and Mn) in the cathode materials of waste lithium batteries to be oxidized, reduced, and dissolved by an oxidant, thereby recovering metal resources. The oxidant can also act as a catalyst to activate the oxidant to generate free radicals, thereby degrading antibiotics. This allows for simultaneous metal recovery and pollutant degradation in a single system.

[0049] 2) The method provided by the present invention is simple to operate, has a high leaching rate of valuable metals, and a high degradation rate of antibiotics; it promotes the coordinated disposal of urban solid waste and wastewater, and has good economic, ecological and environmental benefits;

[0050] 3) The method provided by the present invention for recovering valuable metals from waste lithium batteries and simultaneously degrading antibiotics in water has strong applicability and has a good degradation effect on tetracycline antibiotics, sulfonamide antibiotics, chloramphenicol antibiotics and β-lactam antibiotics, which can meet the treatment needs of antibiotic wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 Schematic diagram of the process for recovering valuable metals from waste lithium batteries and simultaneously degrading antibiotics in water in Examples 1-3;

[0052] Figure 2 is the positive electrode metal leaching rate and antibiotic removal rate in Example 4;

[0053] Figure 3 is the antibiotic removal rate in Example 5;

[0054] Figure 4 is the antibiotic removal rate in Example 6. DETAILED DESCRIPTION

[0055] The present invention is further described in detail below by way of specific examples. Unless otherwise specified, the raw materials, reagents, or devices used in the examples are all commercially available or can be obtained by conventional methods. Unless otherwise specified, all experiments or testing methods are conventional methods in the art.

[0056] Figure 1 Schematic diagram of the process for recovering valuable metals from waste lithium batteries and simultaneously degrading antibiotics in water in Examples 1-3, Figure 1 It can be seen that this method includes discharging and disassembling retired lithium-ion batteries, stripping to obtain waste positive electrode powder, mixing the waste positive electrode powder, an oxidant (peracetic acid) and antibiotic wastewater, carrying out positive electrode metal leaching and antibiotic degradation reactions, adjusting the pH of the leachate after the reaction to carry out a precipitation reaction, filtering and separating to recover the transition metal precipitate and lithium-rich filtrate, adding a precipitant (sodium carbonate solution) to the lithium-rich filtrate to carry out a precipitation reaction again, and precipitating and recovering the lithium-rich precipitate, and after washing and drying, obtaining a lithium-rich product (lithium carbonate).

[0057] Example 1

[0058] This embodiment provides a method for recovering valuable metals from waste lithium manganese oxide batteries and simultaneously degrading antibiotics in water, the steps of which are as follows:

[0059] S11, dismantling the retired lithium manganese oxide battery after discharging it in a saturated sodium chloride solution for 24 hours, and soaking the obtained positive electrode current collector in N-methylpyrrolidone for 12 hours to dissolve the positive electrode binder to obtain the waste lithium manganese oxide positive electrode powder (LiMn2O4);

[0060] S12, adding 0.2 g of waste lithium manganate positive electrode powder to 20 mL of 20 mg / L tetracycline solution, then adding 2 mL of 15% volume concentration peracetic acid, adjusting the system pH to 5, and stirring the reaction at 25°C for 2 hours to obtain a positive electrode metal leaching solution, wherein the leaching rates of lithium and manganese are 99.72% and 99.13%, respectively, and the removal rate of tetracycline is 98.87%;

[0061] S21, adding sodium hydroxide solution to adjust the pH of the positive electrode metal leachate to 12, and performing a precipitation reaction of manganese ions. After reacting for 6 hours, filtering and separating to obtain a lithium-rich filtrate and a manganese precipitate product, wherein the precipitation recovery rate of manganese is 98.54%;

[0062] S31. The lithium-rich solution was placed in a constant temperature magnetic stirring water bath at 95°C, and 4 mL of 5 mol / L sodium carbonate solution was added to carry out lithium precipitation recovery reaction. After the precipitation reaction for 6 hours, the lithium-rich precipitate was filtered and separated and collected, and washed three times with hot water at 95°C. After drying, a lithium carbonate product was obtained, wherein the lithium recovery rate was 94.26%.

[0063] Example 2

[0064] This embodiment provides a method for recovering valuable metals from waste lithium cobalt oxide batteries and simultaneously degrading antibiotics in water, the steps of which are as follows:

[0065] S11, dismantling the retired lithium cobalt oxide battery after discharging it in a saturated sodium chloride solution for 24 hours, and soaking the obtained positive electrode current collector in N-methylpyrrolidone for 12 hours to dissolve the positive electrode binder to obtain the waste lithium cobalt oxide positive electrode powder (LiCoO2);

[0066] S12, adding 0.2 g of waste lithium cobalt oxide positive electrode powder to 20 mL of 20 mg / L tetracycline solution, then adding 2 mL of 15% volume concentration peracetic acid, adjusting the system pH to 5, and stirring the reaction at 25°C for 2 h to obtain a positive electrode metal leaching solution, wherein the leaching rates of lithium and cobalt are 97.52% and 98.53%, respectively, and the removal rate of tetracycline is 95.13%;

[0067] S21, adding sodium hydroxide solution to adjust the pH of the positive electrode metal leachate to 12, and performing a cobalt ion precipitation reaction. After reacting for 6 hours, filtering and separating to obtain a lithium-rich filtrate and a cobalt precipitate product, wherein the cobalt precipitation recovery rate is 99.28%;

[0068] S31. The lithium-rich solution was placed in a constant temperature magnetic stirring water bath at 90° C., 6 mL of 5 mol / L sodium carbonate solution was added, and lithium precipitation recovery reaction was carried out. After the precipitation reaction lasted for 12 hours, the lithium-rich precipitate was collected by filtration and separated, and washed three times with hot water at 90° C. and dried to obtain a lithium carbonate product, wherein the lithium recovery rate was 92.18%.

[0069] Example 3

[0070] This embodiment provides a method for recovering valuable metals from waste lithium nickel cobalt manganese oxide batteries and simultaneously degrading antibiotics in water, the steps of which are as follows:

[0071] S11, put the retired lithium nickel cobalt manganese oxide battery into saturated sodium chloride solution and discharge for 24 hours, then disassemble it, and soak the obtained positive electrode collector in N-methyl pyrrolidone for 12 hours to dissolve the positive electrode binder to obtain the waste lithium nickel cobalt manganese oxide positive electrode powder (LiNi 0.5 Co 0.2 Mn 0.3 O2);

[0072] S12, 0.2 g of waste nickel cobalt manganese oxide positive electrode powder was added to 20 mL of 20 mg / L tetracycline solution, and then 2 mL of 15% volume concentration of peracetic acid was added, the pH of the system was adjusted to 5, and the reaction was stirred at 25 ° C for 2 h to obtain a positive electrode metal leaching solution, wherein the leaching rates of lithium, nickel, cobalt, and manganese were 99.28%, 96.79%, 97.54%, and 99.28%, respectively, and the removal rate of tetracycline was 92.84%;

[0073] S21, adding sodium hydroxide solution to adjust the pH of the positive electrode metal leachate to 12, and performing precipitation reaction of nickel, cobalt, and manganese ions. After reacting for 6 hours, filtering and separating to obtain a lithium-rich filtrate and precipitated products of nickel, cobalt, and manganese, wherein the precipitation recovery rates of nickel, cobalt, and manganese are 98.87%, 99.29%, and 99.59% respectively;

[0074] S31. The lithium-rich solution was placed in a constant temperature magnetic stirring water bath at 90° C., 6 mL of 5 mol / L sodium carbonate solution was added, and lithium precipitation recovery reaction was carried out. After the precipitation reaction lasted for 12 hours, the lithium-rich precipitate was collected by filtration and separated, and washed three times with hot water at 90° C. and dried to obtain a lithium carbonate product, wherein the lithium recovery rate was 90.93%.

[0075] Example 4

[0076] This example explores the effect of the amount of oxidant (peracetic acid) on the positive electrode metal leaching rate and antibiotic removal rate, and the steps are as follows:

[0077] S11, dismantling the retired lithium manganese oxide battery after discharging it in a saturated sodium chloride solution for 24 hours, and soaking the obtained positive electrode current collector in N-methylpyrrolidone for 12 hours to dissolve the positive electrode binder to obtain the waste lithium manganese oxide positive electrode powder;

[0078] S12, prepare 7 portions of 20 mL of 20 mg / L tetracycline solution, add 0.2 g of waste lithium manganate positive electrode powder respectively, and mark them as experimental groups 1-7;

[0079] S13, experimental groups 1-7 were added with 0 mL, 0.25 mL, 0.5 mL, 1.0 mL, 1.5 mL, 2.0 mL, 2.5 mL and 3.0 mL of 15% peracetic acid, respectively, and the pH of the system was adjusted to 5. The mixture was stirred and reacted at 25 ° C for 2 h to obtain the positive electrode metal leaching solution. The leaching rates of lithium and manganese, as well as the removal rate of tetracycline, were detected and calculated respectively.

[0080] Figure 2 is the positive electrode metal leaching rate and antibiotic removal rate in Example 4, Figure 2It can be seen that when the amount of peracetic acid added increases from 0mL to 3mL, the lithium leaching rate increases from 0.25% to 99.67%, the manganese leaching rate increases from 0.18% to 99.29%, and the tetracycline removal efficiency increases from 10.58% to 99.57%. This shows that with the increase in the amount of oxidant used, the leaching rate of the positive electrode metal and the removal rate of the antibiotic both show an upward trend. When the volume concentration of the oxidant is about 15% and the dosage is 10%-15% of the volume of the antibiotic wastewater, the leaching rate of the positive electrode metal and the removal rate of the antibiotic can reach above 99%, which is more conducive to fully realizing the recovery of the positive electrode metal and the degradation of the antibiotic.

[0081] The present invention preferably uses peracetic acid as the oxidant. As a typical reagent commonly used in advanced oxidation processes, peracetic acid has good redox activity and can undergo redox reactions with the phases in the positive electrode of retired lithium batteries to dissolve key metals therein. The dissolved transition metal ions can continue to react with peracetic acid to produce various active oxygen species and organic carbon free radicals such as OH, CH3C(O)O·, CH3C(O)OO·, and CH3OO·, thereby achieving the effect and goal of efficient and simultaneous degradation of antibiotics. Taking lithium cobalt oxide as an example, the chemical reaction equation is as follows:

[0082] 12CH3C(O)OOH+4LiCoO2=4Co(CH3COO)2+4CH3COOLi+7O2+6H2O;

[0083] Co 2+ +CH3C(O)OOH→Co 3+ +CH3C(O)O·+CH3C(O)OO·+·OH;

[0084] CH3C(O)O·+CH3C(O)OO·+·OH+M→CO2+H2O+Intermediates;

[0085] Among them, M represents organic matter and Intermediates represents the intermediate products that may be generated.

[0086] Example 5

[0087] This example explores the effect of the concentration of antibiotic wastewater on the antibiotic removal rate, and the steps are as follows:

[0088] S11, dismantling the retired lithium manganese oxide battery after discharging it in a saturated sodium chloride solution for 24 hours, and soaking the obtained positive electrode current collector in N-methylpyrrolidone for 12 hours to dissolve the positive electrode binder to obtain the waste lithium manganese oxide positive electrode powder;

[0089] S12. Prepare five 20 mL tetracycline solutions with concentrations of 10 mg / L, 20 mg / L, 50 mg / L, 80 mg / L, and 100 mg / L, respectively, and label them as experimental groups 1-5.

[0090] S13. Add 0.2 g of waste lithium manganate positive electrode powder and 2 mL of 15% peracetic acid to experimental groups 1-5 respectively, adjust the system pH to 5, stir and react at 25°C for 2 hours to obtain the positive electrode metal leaching solution, detect and calculate the tetracycline removal rate.

[0091] Figure 3 is the antibiotic removal rate in Example 5, Figure 3 It can be seen that when the concentration of tetracycline increases from 10 mg / L to 100 mg / L, the removal rate decreases from 100% to 78.18%, indicating that the method provided by the present invention has a good degradation effect on antibiotics. When the antibiotic concentration is 10-100 mg / L, the removal rate can be maintained above 75%.

[0092] Example 6

[0093] This example explores the effect of the type of antibiotics in antibiotic wastewater on the antibiotic removal rate, and the steps are as follows:

[0094] S11, dismantling the retired lithium manganese oxide battery after discharging it in a saturated sodium chloride solution for 24 hours, and soaking the obtained positive electrode current collector in N-methylpyrrolidone for 12 hours to dissolve the positive electrode binder to obtain the waste lithium manganese oxide positive electrode powder;

[0095] S12, prepare four 20 mL 20 mg / L antibiotic solutions containing sulfadiazine, cephradine, chloramphenicol, and oxytetracycline, respectively, and label them as experimental groups 1-4;

[0096] S13. Add 0.2 g of waste lithium manganate positive electrode powder and 2 mL of 15% peracetic acid to experimental groups 1-4 respectively, adjust the system pH to 5, stir and react at 25°C for 2 hours to obtain the positive electrode metal leachate, detect and calculate the antibiotic removal rate respectively.

[0097] Figure 4 is the antibiotic removal rate in Example 6, Figure 4 It can be seen that the removal rates of sulfadiazine, cefradine, chloramphenicol and oxytetracycline are 95.49%, 92.18%, 96.27% and 86.26%, respectively, indicating that the method provided by the present invention has a wide range of applications and has a good removal effect on tetracycline antibiotics, sulfonamide antibiotics, chloramphenicol antibiotics and β-lactam antibiotics.

Claims

1. A method for recovering valuable metals from waste lithium batteries and simultaneously degrading antibiotics in water, characterized in that: The following steps are involved: S1. Adding waste lithium battery positive electrode materials and an oxidant to antibiotic wastewater to react and obtain a positive electrode metal leachate; S2, adjusting the pH of the positive electrode metal leachate to 9-14, and performing solid-liquid separation to obtain a lithium-rich filtrate and a transition metal precipitate; S3. Adding a precipitant to the lithium-rich filtrate to undergo precipitation reaction, and collecting the lithium-rich precipitate.

2. The method according to claim 1, characterized in that In step S1, the antibiotic concentration in the antibiotic wastewater is 1-100 mg / L.

3. The method according to claim 2, characterized in that The antibiotics include at least one of tetracycline antibiotics, sulfonamide antibiotics, chloramphenicol antibiotics, and β-lactam antibiotics.

4. The method according to claim 1, wherein In step S1, the amount of the waste lithium battery positive electrode material added is 1-30 g / L.

5. The method according to claim 4, characterized in that The positive electrode material of the waste lithium battery is selected from LiFePO4, LiCoO2, LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.33 Co 0.33 Mn 0.33 O2 or LiMn2O4.

6. The method according to claim 1, characterized in that In step S1, the volume concentration of the oxidant is 10%-20%; The dosage of the oxidant is 5%-15% of the volume of the antibiotic wastewater.

7. The method according to claim 6, characterized in that The oxidant is selected from at least one of peroxyformic acid, peracetic acid, pervaleric acid, perbenzoic acid, and m-chloroperbenzoic acid.

8. The method according to claim 1, characterized in that In step S1, the reaction temperature is 10-90°C, the reaction time is 1-3 hours, and the system pH is 0.1-6.

9. The method according to claim 1, characterized in that In step S3, the concentration of the precipitant is 3-7 mol / L; The dosage of the precipitant is 10%-50% of the volume of the lithium-rich filtrate.

10. The method according to claim 1, characterized in that In step S3, the precipitation reaction temperature is 90-100° C. and the time is 5-15 hours.

Citation Information

Patent Citations

  • Method for recycling valuable metal in waste ternary lithium ion battery

    CN114480852A

Cited By

  • Method for coupling organic wastewater treatment with waste lithium battery recovery

    CN121698510A