Method for improving high-temperature crack resistance of cupronickel alloy based on addition of alterant

By adding copper-magnesium alloy and pure titanium to the copper alloy smelting to refine the grain structure, the problem of high-temperature cracking of copper alloy is solved, and the high-temperature plasticity and crack resistance are improved, ensuring the uniformity and purity of alloy components, and is suitable for fields such as seawater pipelines and heat exchangers.

CN120464891APending Publication Date: 2025-08-12CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510608597.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-13
Publication Date
2025-08-12

AI Technical Summary

Technical Problem

Copper alloys are prone to high-temperature cracking during heating and forging of ingots or hot rolling of slabs, and no effective solution is found in the prior art.

Method used

During the smelting of copper alloy, the copper-magnesium alloy is added as a deoxidant to reduce the oxygen content and remove inclusions. At the same time, pure titanium is added as a deteriorating agent. It is uniformly diffused by stirring, and the grain structure is refined. Combined with heating and slag treatment in the medium frequency or industrial frequency furnace, the uniformity and purity of the alloy composition are ensured.

Benefits of technology

Effectively improve the high-temperature plasticity and crack resistance of copper alloys, reduce the risk of cracking during high-temperature forging or hot rolling, and improve the overall performance consistency and production efficiency of the alloy.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for improving the high-temperature crack resistance of a cupronickel alloy based on addition of an alterant, which comprises the following steps: S1, heating a cupronickel alloy raw material until the cupronickel alloy raw material is completely molten; s2, scum in the metal solution is fished out; s3, adding a copper-magnesium alloy; s4, adding pure titanium, and fully melting and reacting the pure titanium through stirring; s5, scum in the metal solution is fished out; s6, casting after the furnace front analysis is qualified; s7, obtaining a cupronickel alloy round ingot or flat ingot; the copper-magnesium alloy is added as a deoxidizing agent, so that the oxygen content of a metal solution can be reduced, oxygen is prevented from reacting with alloy elements to generate inclusions, the purity of the alloy is improved, and the crack resistance of the alloy is enhanced; the fine and uniform grain structure can effectively improve the high-temperature plasticity of the cupronickel alloy, reduce grain boundary defects, improve the high-temperature crack resistance of the cupronickel alloy and avoid cracking under high-temperature forging or hot rolling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal material processing, in particular to a method for improving the high-temperature crack resistance of white copper alloy by adding a modifier. Background Art

[0002] The characteristics of white copper alloy are good resistance to seawater corrosion and marine biofouling, as well as excellent hot and cold processing properties. White copper alloy products are widely used in seawater pipelines and heat exchangers.

[0003] Although white copper alloy has relatively good hot working properties, high-temperature cracking may occur during the processes of ingot heating and forging or slab hot rolling. Therefore, it is urgent to study a method that can further improve the high-temperature crack resistance of white copper alloy and solve the common problems in the industry.

[0004] Patent CN118127365A discloses a high-strength, wear-resistant copper alloy. Based on the existing aluminum-containing Cu-Ni-based white copper alloy, the auxiliary materials iron and manganese in the traditional alloy are replaced with synthetic ferromanganese boride. Manganese and iron are mixed and borated and added to the copper alloy as ferromanganese boride. This not only further refines the grains, thereby further improving the strength and hardness of the copper alloy, but also enhances the white copper alloy's resistance to high-temperature thermal cracking.

[0005] However, there is no public report on the method of adding titanium as a modifier to white copper alloy to improve high temperature crack resistance. Summary of the Invention

[0006] In view of this, the present invention aims to propose a method for improving the high-temperature cracking resistance of white copper alloy by adding a modifier to solve the problem of high-temperature cracking of white copper alloy during ingot heating forging or slab hot rolling in the prior art.

[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0008] A method for improving the high-temperature crack resistance of white copper alloy by adding a modifier comprises the following steps:

[0009] S1: heating the white copper alloy raw material until it is completely melted;

[0010] S2: remove the scum from the metal solution;

[0011] S3: adding copper-magnesium alloy;

[0012] S4: adding pure titanium and stirring to allow the pure titanium to fully melt and react;

[0013] S5: scoop out the scum from the metal solution;

[0014] S6: After the furnace analysis is qualified, casting is carried out;

[0015] S7: Obtain a white copper alloy round ingot or flat ingot.

[0016] In this application, the addition of copper-magnesium alloy as a deoxidizer can reduce the oxygen content of the metal solution, prevent oxygen from reacting with alloy elements to form inclusions, improve the purity of the alloy, and enhance its crack resistance. The addition of pure titanium as a modifier can refine the grains of the white copper alloy ingot. The fine and uniform grain structure can effectively improve the high-temperature plasticity of the white copper alloy, reduce grain boundary defects, improve the high-temperature crack resistance of the white copper alloy, avoid cracking under high-temperature forging or hot rolling, and reduce the risk of welding cracking, thereby solving common problems in the industry.

[0017] Furthermore, in step S1, the white copper alloy raw material is heated using a medium frequency furnace or an industrial frequency furnace.

[0018] Medium frequency furnaces and industrial frequency furnaces use the principle of electromagnetic induction heating, which can generate an alternating magnetic field in the furnace, causing an induced current to be generated inside the white copper alloy raw material and generate heat. This heating method can make the white copper alloy raw material evenly heated, which is conducive to the full diffusion and fusion of various alloy elements, ensuring the uniformity of the white copper alloy composition, thereby improving the consistency of the alloy performance.

[0019] Furthermore, in step S2, a slag scoop is used to scoop up slag in the metal solution.

[0020] Using a slag scoop to remove slag can effectively remove impurities in the metal solution, improve the purity of the alloy, and thus improve the performance of the alloy.

[0021] Furthermore, in step S3, copper-magnesium alloy is used as a deoxidizer, wherein the mass proportion of magnesium is 0.01 to 0.06%.

[0022] When melting white copper alloy, the oxygen present in the metal solution will react with the alloy elements to form oxide inclusions, reducing the alloy performance. This ratio of copper-magnesium alloy can effectively deoxidize. Magnesium has a strong affinity for oxygen and can preferentially react chemically with oxygen to remove oxygen from the metal solution, reduce oxide inclusions, improve the purity of the alloy, and thereby enhance the strength, toughness, and corrosion resistance of the white copper alloy.

[0023] Furthermore, in step S4, pure titanium is used as a modifier, and in the cupronickel alloy, the mass proportion of the modifier is 0.005-0.1%.

[0024] This setting can effectively refine the grains of the white copper alloy, increase the grain boundaries inside the alloy, and the grain boundaries can hinder the expansion of cracks, thereby improving the strength and toughness of the alloy. At the same time, the refined grains can also improve the high-temperature plasticity of the alloy, reduce the risk of cracks during high-temperature forging and hot rolling, and enhance the alloy's high-temperature crack resistance.

[0025] Furthermore, in step S4, the metal solution is stirred using a stirring rod or electromagnetic stirring.

[0026] This setting allows the modifier to diffuse evenly in the metal solution, ensuring the same content of modifier in each area, thereby making the overall grain refinement effect of the alloy more uniform and improving the consistency of the alloy performance.

[0027] Furthermore, in step S6, during the furnace analysis, when the mass proportion of nickel is 10.15-10.50%, the mass proportion of iron is 1.2-1.70%, and the mass proportion of manganese is 0.70-0.90%, it is determined to be qualified.

[0028] This setting can effectively improve the corrosion resistance, strength and toughness of the alloy.

[0029] Furthermore, in step S7, the obtained cupronickel alloy slab is hot rolled to obtain a cupronickel alloy sheet with a thickness of 10 to 20 mm.

[0030] Flat ingots can be directly processed into plates of specified thickness through hot rolling, which has high production efficiency and can be continuously produced on a large scale to meet market demand.

[0031] Furthermore, in step S7, the obtained white copper alloy ingot is sawn into billets with a length of 175 mm, the billets are homogenized and heated at a temperature of 980°C±10°C, and then the billets are high-temperature forged at a final forging temperature of ≥800°C to obtain rods with a diameter of Ф190.

[0032] The homogenization heating temperature is controlled at 980℃±10℃, which can fully diffuse the alloy elements, eliminate the component segregation produced during the casting process, make the structure of the white copper alloy ingot uniform, and improve the stability of the internal structure of the material. The final forging temperature of ≥800℃ can ensure that the billet always maintains good plasticity during the forging process, making the forging process smoother, reducing forging defects, and improving the quality and yield of the bar.

[0033] Compared with the prior art, the method of improving the high-temperature crack resistance of white copper alloy by adding a modifier according to the present invention has the following advantages:

[0034] Adding copper-magnesium alloy as a deoxidizer can reduce the oxygen content of the metal solution, prevent oxygen from reacting with alloy elements to form inclusions, improve the purity of the alloy, and enhance its crack resistance. Adding pure titanium as a modifier can refine the grains of the white copper alloy ingot. The fine and uniform grain structure can effectively improve the high-temperature plasticity of the white copper alloy, reduce grain boundary defects, improve the high-temperature crack resistance of the white copper alloy, avoid cracking under high-temperature forging or hot rolling, and reduce the risk of welding cracking, solving common problems in the industry. DETAILED DESCRIPTION

[0035] To make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the embodiments. It should be understood that the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The specific embodiments described herein are merely for explaining the present invention and are not intended to limit the present invention. It should be noted that, unless there is a conflict, the features in the embodiments and embodiments of the present invention may be combined with each other.

[0036] Example 1

[0037] The present invention has been applied to the production of hot-rolled plates from BFe10-1.6-1 white copper alloy flat ingots, and the specific steps are as follows:

[0038] A1: Alloy and smelt the BFe10-1.6-1 white copper alloy raw material in a medium frequency furnace or an industrial frequency furnace until it is completely melted;

[0039] A2: Use a slag scoop to remove the slag from the metal solution;

[0040] A3: Add copper-magnesium alloy for deoxidation, where the mass proportion of magnesium is 0.02%;

[0041] A4: Add pure titanium to the cupronickel solution, with the mass proportion of pure titanium being 0.07%. Then use a stirring rod to stir the metal solution to ensure that the pure titanium fully dissolves and reacts.

[0042] A5: Use a slag scoop to remove the slag from the metal solution;

[0043] A6: After the furnace analysis is qualified, casting can be carried out;

[0044] A7: Obtain a BFe10-1.6-1 copper-nickel alloy flat ingot;

[0045] A8: The cupronickel alloy flat ingot is hot-rolled at high temperature to be processed into cupronickel alloy plates with a thickness of 10 to 20 mm.

[0046] Specifically, in step A6, when the main components are analyzed before the furnace, when the mass proportion of nickel is 10.15-10.50%, the mass proportion of iron is 1.56-1.70%, and the mass proportion of manganese is 0.70-0.90%, it is determined to be qualified.

[0047] The BFe10-1.6-1 white copper alloy slab obtained by casting in Example 1 did not crack during the hot rolling process, and the product had good high-temperature crack resistance.

[0048] Example 2

[0049] The present invention has been applied to the forging process of BFe10-1-1 white copper alloy round ingot products with a diameter of 145 mm. The specific steps are as follows:

[0050] B1: Alloy and smelt the BFe10-1-1 white copper alloy raw material in a medium frequency furnace or an industrial frequency furnace until it is completely melted;

[0051] B2: Use a slag scoop to remove slag from the metal solution;

[0052] B3: Add copper-magnesium alloy for deoxidation, where the mass proportion of magnesium is 0.03%;

[0053] B4: Add pure titanium to the cupronickel solution, with the mass proportion of pure titanium being 0.01%. Then use a stirring rod to stir the metal solution to allow the pure titanium to fully dissolve and react.

[0054] B5: Use a slag scoop to remove slag from the metal solution;

[0055] B6: After the furnace analysis is qualified, casting can be carried out;

[0056] B7: Obtain a BFe10-1-1 white copper alloy ingot;

[0057] B8: Saw the ingot into billets with a length of 175 mm;

[0058] B8: Homogenize the blank to a temperature of 980°C ± 10°C. When the blank is charged at the desired temperature, the blank should be kept warm for ≥ 1 hour. When the blank is heated with the furnace, the blank should be kept warm for 30 to 45 minutes.

[0059] B9: Forging the blank at high temperature, with the final forging temperature ≥800℃;

[0060] B10: Obtain a rod with a diameter of Ф190.

[0061] In step B6, when the main components are analyzed before the furnace, it is determined to be acceptable when the mass proportion of nickel is 10.15-10.50%, the mass proportion of iron is 1.2-1.6%, and the mass proportion of manganese is 0.70-0.90%.

[0062] In step B9, the forging equipment uses an air forging hammer or a free forging press that matches the weight of the billet. During forging, a light hammer is used for fast hitting in the initial stage, a heavy hammer is used for slow hitting in the middle stage, and a light hammer is used for fast hitting in the final stage. After forging is completed, the billet forging ratio is not less than 3.

[0063] In the initial stage, light hammering and fast beating are used to allow the blank to gradually adapt to deformation under a smaller impact force, which can avoid cracks caused by sudden excessive pressure and preliminarily improve the surface quality of the blank; in the middle stage, heavy hammering and slow beating are used to give the blank enough deformation, making the internal structure denser, refining the grains, and effectively improving the mechanical properties of the alloy; in the finishing stage, light hammering and fast beating can be used to finely trim the blank when it is close to the finished product size, control the dimensional accuracy, and eliminate the residual stress caused by forging, thereby ensuring the dimensional accuracy and performance stability of the product.

[0064] After forging, the forging ratio of the billet is not less than 3, which can enable the billet to have sufficient plastic deformation. A larger forging ratio can crush coarse grains and significantly improve the strength, toughness and fatigue resistance of the product.

[0065] Let me explain here that the forging ratio is a way to express the degree of metal deformation, which is equal to the ratio of the cross-sectional area of the billet before forging to the cross-sectional area of the billet after forging, or the ratio of the height of the billet before and after deformation.

[0066] After each forging, check that there are no cracks or cracks on the surface of the forging.

[0067] The BFe10-1-1 white copper alloy Ø145 ingot obtained by casting in Example 2 was forged to obtain a rod with a diameter of Ø190. No cracking occurred during the forging process, and the product had good high-temperature crack resistance.

[0068] This application solves the common problems in the industry by adding a certain amount of pure titanium as a modifier in the smelting process of the white copper alloy to refine the grains of the white copper alloy ingot, effectively improve the high-temperature plasticity of the white copper alloy, avoid cracking under high-temperature forging or hot rolling, reduce the risk of welding cracking, and thus solve the common problems in the industry.

[0069] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined by the claims.

Claims

1. A method for improving the high temperature crack resistance of white copper alloy by adding a modifier, characterized in that: Including steps: S1: heating the white copper alloy raw material until it is completely melted; S2: remove the scum from the metal solution; S3: adding copper-magnesium alloy; S4: adding pure titanium and stirring to allow the pure titanium to fully melt and react; S5: scoop out the scum from the metal solution; S6: After the furnace analysis is qualified, casting is carried out; S7: Obtain a white copper alloy round ingot or flat ingot.

2. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S1, a medium frequency furnace or an industrial frequency furnace is used to heat the white copper alloy raw material.

3. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S2, a slag scoop is used to scoop up slag in the molten metal.

4. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S3, copper-magnesium alloy is used as a deoxidizer, wherein the mass proportion of magnesium is 0.01-0.06%.

5. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S4, pure titanium is used as a modifier, and the mass proportion of the modifier in the white copper alloy is 0.005-0.1%.

6. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S4, the metal solution is stirred using a stirring rod or electromagnetic stirring.

7. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S6 , when the furnace analysis shows that the mass percentage of nickel is 10.15-10.50%, the mass percentage of iron is 1.2-1.70%, and the mass percentage of manganese is 0.70-0.90%, it is determined to be acceptable.

8. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S7, the obtained cupronickel alloy slab is hot rolled to obtain a cupronickel alloy sheet with a thickness of 10 to 20 mm.

9. The method for improving high temperature crack resistance of white copper alloy by adding a modifier according to claim 1, characterized in that: In step S7, the obtained white copper alloy ingot is sawn into billets with a length of 175 mm, the billets are homogenized and heated at a temperature of 980°C±10°C, and then the billets are high-temperature forged at a final forging temperature of ≥800°C to obtain rods with a diameter of Ф190.

Citation Information

Cited By

  • Method for improving thermal cracking resistance of cupronickel alloy without adding alterant

    CN121183152A

  • Zirconium-containing B10 copper-nickel alloy and preparation method thereof

    CN122038844A