Yttrium modified aluminide composite coating as well as preparation method and application thereof

The preparation of yttrium modified aluminide composite coating on the surface of nickel-based high-temperature alloy by chemical vapor deposition method, solving the problem of uneven deposition of the modified coating on the surface of nickel-based alloy, and achieving uniform coating preparation and high-temperature protection performance improvement on the inner surface of complex and slender tubular components.

CN120591720APending Publication Date: 2025-09-05NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410251080.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2025-09-05

AI Technical Summary

Technical Problem

In the prior art, uniform deposition of the modified coating on the surface of nickel-based alloy is difficult to achieve, especially on the inner surface of complex and elongated tubular components, and traditional methods are prone to cause defects such as powder hole blockage.

Method used

The chemical vapor deposition method is used to react the activation gas with the yttrium source and the aluminum source on the surface of the nickel-based high-temperature alloy matrix to form a gas-phase halide, and the temperature is controlled to 950-1050°C to form a yttrium modified aluminide composite coating with an interdiffusion layer and an yttrium-rich layer.

Benefits of technology

It achieves uniform deposition of dense coating on the surface of nickel-based high-temperature alloy, improves the bonding strength and high-temperature protection performance of the coating, adapts to the coating preparation of complex-shaped parts, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120591720A_ABST
    Figure CN120591720A_ABST
Patent Text Reader

Abstract

The invention discloses an yttrium modified aluminide composite coating as well as a preparation method and application thereof. The preparation method comprises the following steps: placing a nickel-based high-temperature alloy matrix in a reaction chamber of chemical vapor deposition equipment; respectively reacting the activated gas with a yttrium source and an aluminum source to prepare a gas-phase halide of yttrium and a gas-phase halide of aluminum; the temperature of the reaction chamber is increased to 950-1050 DEG C, carrier gas, the yttrium gas-phase halide and the aluminum gas-phase halide are introduced into the reaction chamber and react with the base body, and therefore the yttrium modified aluminide composite coating is formed on the nickel-based superalloy base body in a deposition mode; wherein the yttrium modified aluminide composite coating comprises an interdiffusion layer and a yttrium-rich layer which are sequentially formed on the surface of a matrix. The yttrium modified aluminide composite coating prepared through the method is compact in structure, and meanwhile the preparation method of the yttrium modified aluminide composite coating is high in production efficiency, convenient to operate and capable of adapting to uniform coating of the surfaces of parts in complex shapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material surface treatment, and particularly relates to an yttrium-modified aluminide composite coating and a preparation method and application thereof. Background Art

[0002] With the continuous development of modern aircraft engines and gas turbines, the protection requirements for engine blade materials have also increased. However, nickel-based superalloys, a common material for hollow engine blades, are no longer able to meet the protection requirements of the engine's gas inlet. Therefore, applying a high-temperature protective coating to the surface of the material is an effective means of increasing the operating temperature of nickel-based superalloys. Since the 1950s, aluminized coatings have been widely used on nickel-based and cobalt-based superalloy turbine blades and guide vanes. Today, with the continuous advancement of technology, single aluminide coatings are no longer able to meet the increasingly stringent protection requirements of high-temperature components. Therefore, the addition of the modified rare earth element yttrium to the coating is often used to adjust and improve the coating structure and thus optimize the material's high-temperature protection performance. However, the large atomic radius of yttrium means that it is difficult for it to enter nickel aluminide, so the preparation process of yttrium-modified aluminide coatings has always been a focus of research. When it comes to coating the inner surfaces of complex, slender tubular components, traditional methods like embedded infiltration are prone to defects such as powder pore clogging. Chemical vapor deposition (CVD), which can coat surfaces of complex shapes, still has certain technical limitations. This is particularly true for uniform deposition of modified coatings on nickel-based alloy surfaces. Summary of the Invention

[0003] The main purpose of the present invention is to provide a yttrium-modified aluminide composite coating and its preparation method and application, so as to overcome the deficiency of the prior art that the modified coating is difficult to be uniformly deposited and prepared on the surface of nickel-based alloy.

[0004] To achieve the aforementioned object of the invention, the technical solutions adopted by the present invention include:

[0005] An embodiment of the present invention provides a method for preparing a yttrium-modified aluminide composite coating, which comprises:

[0006] placing a nickel-based high-temperature alloy substrate in a reaction chamber of a chemical vapor deposition device;

[0007] The activated gas is reacted with the yttrium source and the aluminum source to produce a gas-phase halide of yttrium and a gas-phase halide of aluminum;

[0008] The reaction chamber is heated to 950-1050° C., a carrier gas, the yttrium gas halide, and the aluminum gas halide are introduced into the reaction chamber to react with the substrate, thereby depositing a yttrium-modified aluminide composite coating on the nickel-based high-temperature alloy substrate;

[0009] The yttrium-modified aluminide composite coating comprises an interdiffusion layer and a yttrium-rich layer sequentially formed on the surface of a substrate.

[0010] The embodiment of the present invention also provides a yttrium-modified aluminide composite coating prepared by the aforementioned preparation method.

[0011] The embodiment of the present invention also provides the use of the aforementioned yttrium-modified aluminide composite coating in the surface protection of engine blade materials.

[0012] An embodiment of the present invention further provides a surface modification method for a nickel-based high-temperature alloy, comprising: preparing an yttrium-modified aluminide composite coating on the surface of the nickel-based high-temperature alloy using the aforementioned method, thereby achieving modification of the nickel-based high-temperature alloy.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] (1) The XRD test results of the yttrium-modified aluminide composite coating prepared by the present invention show that the coating is mainly composed of β-NiAl phase, which can provide Al elements for the formation and repair of the surface oxide film of the hollow blade during service, thereby effectively extending its service life;

[0015] (2) The preparation method provided by the present invention can obtain yttrium-modified aluminide composite coatings of different thicknesses by regulating the process temperature and treatment time. It has high production efficiency, is easy to operate, and can be adapted to prepare uniform coatings on the inner surfaces of complex, slender tubular components.

[0016] (3) The yttrium-modified aluminide composite coating prepared by the present invention has a dense structure and good bonding strength with the substrate, and can be used for the protection of nickel-based high-temperature alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0018] Figure 1 This is a scanning electron microscope (SEM) image of the cross section of the yttrium-modified aluminide composite coating prepared on the surface of the nickel-based high-temperature alloy at a deposition temperature of 950° C. in Example 1 of the present invention.

[0019] Figure 2 1 is an XRD pattern of the yttrium-modified aluminide composite coating prepared on a nickel-based high-temperature alloy substrate using different processes in Examples 1-3 of the present invention;

[0020] Figure 3is a scanning electron microscope (SEM) image of a cross section of a yttrium-modified aluminide composite coating prepared on the surface of a nickel-based high-temperature alloy at a deposition temperature of 1000° C. in Example 2 of the present invention;

[0021] Figure 4 is a scanning electron microscope (SEM) image of a cross section of a yttrium-modified aluminide composite coating prepared on the surface of a nickel-based high-temperature alloy at a deposition temperature of 1050° C. in Example 3 of the present invention;

[0022] Figure 5 This is a scanning electron microscope (SEM) image of the cross section of a single aluminide coating in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0023] In view of the shortcomings of the prior art, the inventors of this case, after long-term research and extensive practice, have proposed the technical solution of the present invention. The technical solution of the present invention will be clearly and completely described below. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by persons of ordinary skill in the art without making any creative effort shall fall within the scope of protection of the present invention.

[0024] Specifically, as one aspect of the technical solution of the present invention, a method for preparing a yttrium-modified aluminide composite coating includes:

[0025] placing a nickel-based high-temperature alloy substrate in a reaction chamber of a chemical vapor deposition device;

[0026] The activated gas is reacted with the yttrium source and the aluminum source to produce a gas-phase halide of yttrium and a gas-phase halide of aluminum;

[0027] The reaction chamber is heated to 950-1050° C., a carrier gas, the yttrium gas halide, and the aluminum gas halide are introduced into the reaction chamber to react with the substrate, thereby depositing a yttrium-modified aluminide composite coating on the nickel-based high-temperature alloy substrate;

[0028] The yttrium-modified aluminide composite coating comprises an interdiffusion layer and a yttrium-rich layer sequentially formed on the surface of a substrate.

[0029] In some preferred embodiments, the phases of the interdiffusion layer include NiAl intermetallic compound, σ-Cr3Ni2 precipitation phase and Cr7C3 precipitation phase.

[0030] In some preferred embodiments, the physical phase of the yttrium-rich layer includes a β-NiAl phase and a yttrium-rich phase, wherein the yttrium-rich phase is distributed in the β-NiAl phase in a needle shape, and the β-NiAl phase is the main phase structure of the yttrium-rich layer.

[0031] In some preferred embodiments, the thickness of the interdiffusion layer is 4.56 to 9.16 μm.

[0032] In some preferred embodiments, the thickness of the yttrium-rich layer is 8.17 to 13.62 μm.

[0033] In some preferred embodiments, the preparation method specifically includes: placing a yttrium source in an external reaction device, then introducing an activated gas and reacting at 250-400° C. to obtain a gas-phase halide of yttrium.

[0034] Furthermore, the yttrium source includes yttrium alloy powder, but is not limited thereto.

[0035] Furthermore, the chemical formula of the gas phase halide of yttrium is YCl3.

[0036] In some preferred embodiments, the preparation method specifically includes: placing an aluminum source in an external reaction device, then introducing an activated gas and reacting at 250-400° C. to produce a gas-phase halide of aluminum.

[0037] Furthermore, the aluminum source includes aluminum particles, but is not limited thereto.

[0038] Furthermore, the chemical formula of the gas phase aluminum halide is A1Cl n , where n is 1 to 3.

[0039] In some preferred embodiments, the activation gas includes HCl gas, but is not limited thereto.

[0040] In some preferred embodiments, the carrier gas includes Ar and / or H2, but is not limited thereto.

[0041] In some preferred embodiments, the preparation method specifically comprises:

[0042] placing a nickel-based high-temperature alloy substrate in a reaction chamber of a chemical vapor deposition device;

[0043] The air in the reaction chamber is extracted and then the carrier gas is introduced;

[0044] When the temperature in the reaction chamber rises to 950-1050° C., the gaseous halide of yttrium and the gaseous halide of aluminum are introduced into the reaction chamber by a carrier gas and react with the substrate, thereby depositing a yttrium-modified aluminide composite coating on the nickel-based high-temperature alloy substrate.

[0045] In some preferred embodiments, the preparation method of the yttrium-modified aluminide composite coating includes: using an improved chemical vapor deposition (CVD) system to perform aluminization on the surface of a nickel-based high-temperature alloy, thereby obtaining a yttrium-modified aluminide composite coating with a double-layer structure on the nickel-based high-temperature alloy substrate.

[0046] The specific process is as follows: a CVD system with two sets of external precursor generators is used, and donor materials containing pre-deposited elements yttrium and aluminum are respectively loaded into the external generators. First, the activated gas is introduced into the external generator and reacts with the donor material at a certain temperature to generate gaseous halides of yttrium and aluminum. These gaseous halides are then carried into the CVD chamber by protective gas, and exothermic reactions occur with the substrate at different deposition temperatures and times. Yttrium and aluminum elements are deposited on the surface of the nickel-based high-temperature alloy and solid-phase diffusion occurs, eventually forming an yttrium-modified aluminide composite coating on the surface of the nickel-based high-temperature alloy substrate.

[0047] Preferably, the nickel-based high-temperature alloy needs to be pre-treated to remove surface contaminants and burrs, and cleaned and dried.

[0048] Preferably, the donor material loaded with pre-deposition elements is pure Al particles and Y alloy powder, which are used to provide the coating deposition elements Al and Y for the aluminide coating.

[0049] Preferably, the activated gas introduced into the external generator is HCl gas.

[0050] Preferably, the temperature at which the activated gas is introduced into the external generator and reacts with the donor material to generate gaseous halide at a certain temperature is 250-400°C.

[0051] As an option, the protective gas is Ar / H2, which acts as a carrier gas to transport the gaseous halide AlCl n and YCl3 are carried into the CVD chamber.

[0052] Preferably, the deposition temperature for exothermic reaction with the substrate at different deposition temperatures is 950°C to 1050°C.

[0053] The present invention proposes a method for uniformly preparing a yttrium-modified coating on the surface of a nickel-based alloy using a chemical vapor deposition process. The yttrium-modified aluminide coating obtained by performing an aluminizing process on the surface of the nickel-based high-temperature alloy material can more efficiently provide Al elements for the repair of the coating during service.

[0054] Another aspect of the embodiments of the present invention further provides a yttrium-modified aluminide composite coating prepared by the aforementioned preparation method.

[0055] Another aspect of the embodiments of the present invention further provides the use of the aforementioned yttrium-modified aluminide composite coating in the surface protection of engine blade materials.

[0056] Specifically, the invention relates to preparing a yttrium-modified aluminide coating on the inner surface of the elongated hole of the hollow blade of the aircraft engine turbine.

[0057] The aluminized coating prepared by the present invention can promote the diffusion process of Al in p-NiAl, thereby more efficiently providing Al elements for the repair of the coating during service.

[0058] Another aspect of an embodiment of the present invention further provides a surface modification method for a nickel-based high-temperature alloy, comprising: preparing an yttrium-modified aluminide composite coating on the surface of the nickel-based high-temperature alloy using the aforementioned method, thereby achieving modification of the nickel-based high-temperature alloy.

[0059] The yttrium-modified aluminide composite coating prepared by the present invention has a dense structure. Meanwhile, the preparation method of the yttrium-modified aluminide composite coating has high production efficiency, is easy to operate, and can adapt to uniform coating on the surface of components with complex shapes.

[0060] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and the accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0061] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0062] Example 1

[0063] (1) The substrate is made of nickel-based high-temperature alloy. It is first polished with sandpaper until the surface is bright and smooth, then ultrasonically cleaned with alcohol, and finally soaked and dried with alcohol.

[0064] (2) The pre-treated alloy substrate is placed in a CVD chamber. Two sets of external generators are loaded with pure Al particles and Y alloy powder, which are donor materials containing pre-deposited elements. HCl activation gas is introduced into the external generators. At 300°C, the pure Al particles and Y alloy powder react with the HCl gas to form gaseous halides AlCl3 and YCl3. The air in the CVD chamber is evacuated and then introduced with a carrier gas. When the temperature rises to 950°C, AlCl3 and YCl3 are then carried into the CVD chamber by Ar / H2 and react exothermically with the surface of the nickel-based alloy substrate to form a yttrium-modified aluminide coating.

[0065] (3) The deposition time in the CVD chamber is 1.5 h.

[0066] (4) After the deposition is completed, the heating is stopped and the sample is taken out of the furnace after cooling to room temperature according to a certain cooling process.

[0067] (5) After the aluminide coating is deposited, tail gas is generated, which contains waste gases such as H2, HCl, and AlCl3. These waste gases are pumped into an alkaline aqueous solution by a vacuum pump to remove HCl and AlCl3 gases, and the remaining gases are discharged into the atmosphere.

[0068] (6) The cross-sectional morphology of the yttrium-modified aluminide composite coating prepared on the surface of nickel-based high-temperature alloy by CVD method at a deposition temperature of 950°C is as follows: Figure 1 The prepared coating was subjected to XRD test, and the results showed that the yttrium-modified aluminide composite coating prepared under this process was β-NiAl phase, as shown in Figure 2 As shown. Figure 1 The cross-sectional morphology is shown to be a two-layer structure: the outer layer (OL) is the coating, primarily composed of β-NiAl and a gray yttrium-rich phase; the inner layer (IDL) is the interdiffusion layer, primarily composed of NiAl intermetallic compounds and precipitated phases. Under these process conditions, the coating thickness is approximately 8.17 μm, and the interdiffusion layer thickness is approximately 4.56 μm.

[0069] (7) The diffusion coefficient of Al in β-NiAl at 950°C after adding the modifying element yttrium obtained by the first principles method is shown in Table 1. It is obvious that the addition of yttrium promotes the diffusion process of Al in β-NiAl.

[0070] Example 2

[0071] (1) The substrate is made of nickel-based high-temperature alloy. It is first polished with sandpaper until the surface is bright and smooth, then ultrasonically cleaned with alcohol, and finally soaked and dried with alcohol.

[0072] (2) The pre-treated alloy substrate is placed in a CVD chamber. Two sets of external generators are loaded with pure Al particles and Y alloy powder, which are donor materials containing pre-deposited elements. HCl activation gas is introduced into the external generators. At 300°C, the pure Al particles and Y alloy powder react with the HCl gas to form gaseous halides AlCl3 and YCl3. The air in the CVD chamber is evacuated and then introduced with a carrier gas. When the temperature rises to 1000°C, AlCl3 and YCl3 are then carried into the CVD chamber by Ar / H2 and react exothermically with the surface of the nickel-based alloy substrate to form a yttrium-modified aluminide coating.

[0073] (3) The deposition time in the CVD chamber is 1.5 h.

[0074] (4) After the deposition is completed, the heating is stopped and the sample is taken out of the furnace after cooling to room temperature according to a certain cooling process.

[0075] (5) After the aluminide coating is deposited, tail gas is generated, which contains waste gases such as H2, HCl, and AlCl3. These waste gases are pumped into an alkaline aqueous solution by a vacuum pump to remove HCl and AlCl3 gases, and the remaining gases are discharged into the atmosphere.

[0076] (6) The cross-sectional morphology of the yttrium-modified aluminide composite coating prepared on the surface of nickel-based high-temperature alloy by CVD method at a deposition temperature of 1000℃ is as follows: Figure 3 The prepared coating was subjected to XRD test, and the results showed that the yttrium-modified aluminide composite coating prepared under this process was β-NiAl phase, as shown in Figure 2 As shown. Figure 3 The cross-sectional morphology is shown to be a two-layer structure: the outer layer (OL) is the coating, primarily composed of β-NiAl and a gray yttrium-rich phase; the inner layer (IDL) is the interdiffusion layer, primarily composed of NiAl intermetallic compounds and precipitated phases. Under these process conditions, the coating thickness is approximately 11.07 μm, and the interdiffusion layer thickness is approximately 8.36 μm.

[0077] (7) The diffusion coefficient of Al in β-NiAl at 1000°C after adding the modifying element yttrium obtained by the first principles method is shown in Table 1. It is obvious that the addition of yttrium promotes the diffusion process of Al in β-NiAl.

[0078] Example 3

[0079] (1) The substrate is made of nickel-based high-temperature alloy. It is first polished with sandpaper until the surface is bright and smooth, then ultrasonically cleaned with alcohol, and finally soaked and dried with alcohol.

[0080] (2) The pre-treated alloy substrate is placed in a CVD chamber. Two sets of external generators are loaded with pure Al particles and Y alloy powder, which are donor materials containing pre-deposited elements. HCl activation gas is introduced into the external generators. At 300°C, the pure Al particles and Y alloy powder react with the HCl gas to form gaseous halides AlCl3 and YCl3. The air in the CVD chamber is evacuated and then introduced with a carrier gas. When the temperature rises to 1050°C, AlCl3 and YCl3 are then carried into the CVD chamber by Ar / H2 and react exothermically with the surface of the nickel-based alloy substrate to form a yttrium-modified aluminide coating.

[0081] (3) The deposition time in the CVD chamber is 1.5 h.

[0082] (4) After the deposition is completed, the heating is stopped and the sample is taken out of the furnace after cooling to room temperature according to a certain cooling process.

[0083] (5) After the aluminide coating is deposited, tail gas is generated, which contains waste gases such as H2, HCl, and AlCl3. These waste gases are pumped into an alkaline aqueous solution by a vacuum pump to remove HCl and AlCl3 gases, and the remaining gases are discharged into the atmosphere.

[0084] (6) The cross-sectional morphology of the yttrium-modified aluminide composite coating prepared on the surface of nickel-based high-temperature alloy by CVD method at a deposition temperature of 1050°C is as follows: Figure 4 The prepared coating was subjected to XRD test, and the results showed that the yttrium-modified aluminide composite coating prepared under this process was β-NiAl phase, as shown in Figure 2 As shown. Figure 4 The cross-sectional morphology is shown to be a two-layer structure: the outer layer (OL) is the coating, primarily composed of β-NiAl and a gray yttrium-rich phase; the inner layer (IDL) is the interdiffusion layer, primarily composed of NiAl intermetallic compounds and precipitated phases. Under these process conditions, the coating thickness is approximately 13.62 μm, and the interdiffusion layer thickness is approximately 9.16 μm.

[0085] (7) The diffusion coefficient of Al in β-NiAl at 1050°C after adding the modifying element yttrium obtained by the first principles method is shown in Table 1. It is obvious that the addition of yttrium promotes the diffusion process of Al in β-NiAl.

[0086] Comparative Example 1

[0087] (1) The substrate is made of nickel-based high-temperature alloy. It is first polished with sandpaper until the surface is bright and smooth, then ultrasonically cleaned with alcohol, and finally soaked and dried with alcohol.

[0088] (2) The pre-treated alloy substrate is placed in a CVD chamber. Pure Al particles, a donor material containing pre-deposited elements, are loaded into an external generator. HCl activation gas is introduced into the external generator. At 300°C, the pure Al particles react with the HCl gas to form a gaseous halide, AlCl3. The AlCl3 is then carried into the CVD chamber via Ar / H2 and exothermically reacts with the surface of the nickel-based alloy substrate at a deposition temperature of 1050°C, forming a single aluminide coating.

[0089] (3) The deposition time in the CVD chamber is 1.5 h.

[0090] (4) After the deposition is completed, the heating is stopped and the sample is taken out of the furnace after cooling to room temperature according to a certain cooling process.

[0091] (5) After the aluminide coating is deposited, tail gas is generated, which contains waste gases such as H2, HCl, and AlCl3. These waste gases are pumped into an alkaline aqueous solution by a vacuum pump to remove HCl and AlCl3 gases, and the remaining gases are discharged into the atmosphere.

[0092] (6) The cross-sectional morphology of a single aluminide coating prepared on a nickel-based high-temperature alloy surface by CVD at a deposition temperature of 1050°C is shown in Figure 2. Figure 5 The prepared coating was subjected to XRD test, and the results showed that the single aluminide coating prepared under this process was β-NiAl phase, as shown in Figure 2 As shown. Figure 5 The cross-sectional morphology is shown to be a two-layer structure: the outer layer (OL) is the coating, primarily composed of the β-NiAl phase; the inner layer (IDL) is the interdiffusion layer, primarily composed of NiAl intermetallic compounds and precipitated phases. Under these process conditions, the coating thickness is approximately 15.72 μm, and the interdiffusion layer thickness is approximately 11.96 μm.

[0093] (7) The diffusion coefficient of Al in β-NiAl without the addition of the modifying element yttrium at 1050°C obtained by the first principles method is shown in Table 1. It is obvious that the diffusion coefficient of Al in β-NiAl without the addition of yttrium is lower.

[0094] Table 1 Characterization data of Examples 1-3 and Comparative Example 1

[0095]

[0096] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments using other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0097] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical variations made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the scope of protection of the present invention.

Claims

1. A method for preparing a yttrium-modified aluminide composite coating, characterized in that: include: placing a nickel-based high-temperature alloy substrate in a reaction chamber of a chemical vapor deposition device; The activated gas is reacted with the yttrium source and the aluminum source to produce a gas-phase halide of yttrium and a gas-phase halide of aluminum; The reaction chamber is heated to 950-1050° C., a carrier gas, the yttrium gas halide, and the aluminum gas halide are introduced into the reaction chamber to react with the substrate, thereby depositing a yttrium-modified aluminide composite coating on the nickel-based high-temperature alloy substrate; The yttrium-modified aluminide composite coating comprises an interdiffusion layer and a yttrium-rich layer sequentially formed on the surface of a substrate.

2. The preparation method according to claim 1, wherein: The phases of the interdiffusion layer include NiAl intermetallic compound, σ-Cr3Ni2 precipitation phase and Cr7C3 precipitation phase; And / or, the physical phase of the yttrium-rich layer includes a β-NiAl phase and a yttrium-rich phase, wherein the yttrium-rich phase is distributed in the β-NiAl phase in a needle shape.

3. The preparation method according to claim 1, wherein: The thickness of the interdiffusion layer is 4.56 to 9.16 μm; And / or, the thickness of the yttrium-rich layer is 8.17-13.62 μm.

4. The preparation method according to claim 1, characterized in that Specifically include: A yttrium source is placed in an external reaction device, and then an activated gas is introduced and reacted at 250-400°C to obtain a gas-phase halide of yttrium; preferably, the yttrium source includes yttrium alloy powder; preferably, the chemical formula of the gas-phase halide of yttrium is YCl3.

5. The preparation method according to claim 1, characterized in that Specifically include: An aluminum source is placed in an external reaction device, and then an activated gas is introduced and reacted at 250-400°C to obtain a gaseous halide of aluminum. Preferably, the aluminum source comprises aluminum particles. Preferably, the chemical formula of the gaseous halide of aluminum is AlCl n , where n is 1 to 3.

6. The preparation method according to claim 1, wherein: The activation gas includes HCl gas; and / or the carrier gas includes Ar and / or H2.

7. The preparation method according to claim 1, characterized in that Specifically include: placing a nickel-based high-temperature alloy substrate in a reaction chamber of a chemical vapor deposition device; The air in the reaction chamber is extracted and then the carrier gas is introduced; When the temperature in the reaction chamber rises to 950-1050° C., the gaseous halide of yttrium and the gaseous halide of aluminum are introduced into the reaction chamber by a carrier gas and react with the substrate, thereby depositing a yttrium-modified aluminide composite coating on the nickel-based high-temperature alloy substrate.

8. A yttrium-modified aluminide composite coating prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the yttrium-modified aluminide composite coating according to claim 8 in surface protection of engine blade materials.

10. A surface modification method for a nickel-based high-temperature alloy, characterized in that: include: The method according to any one of claims 1 to 7 is used to prepare a yttrium-modified aluminide composite coating on the surface of a nickel-based high-temperature alloy, thereby achieving modification of the nickel-based high-temperature alloy.