Nanocrystalline barium titanate ceramic dielectric material as well as preparation method and application thereof

By using magnesium source, aluminum source or silicon source as grain growth inhibitor, nanocrystalline barium titanate ceramic dielectric material is prepared under normal pressure by solid phase coating method, which solves the problem of grain size control and realizes efficient preparation of nanocrystalline materials suitable for multilayer ceramic capacitors, meeting the requirements of high capacity and small size.

CN120613227APending Publication Date: 2025-09-09SHENZHEN INST OF ADVANCED TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510914999.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-03
Publication Date
2025-09-09

AI Technical Summary

Technical Problem

In the existing technology, the grain size of nanocrystalline barium titanate ceramic dielectric materials cannot be effectively controlled, which affects the dielectric properties of the ceramics and causes environmental pollution problems, making it difficult to meet the needs of high-capacity, small-size multilayer ceramic capacitors.

Method used

A magnesium source, an aluminum source or a silicon source is used as a grain growth inhibitor, and a simple solid-phase coating method is used to inhibit grain growth during pressureless sintering to prepare a nanocrystalline barium titanate ceramic dielectric material. Appropriate molar percentages and combinations are selected to control grain size.

Benefits of technology

Nanocrystalline barium titanate ceramic dielectric materials with small and uniform grains were prepared, which are suitable for multilayer ceramic capacitors. The process is simple, low-cost, environmentally friendly, and suitable for large-scale industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120613227A_ABST
    Figure CN120613227A_ABST
Patent Text Reader

Abstract

The invention relates to a nanocrystalline barium titanate ceramic dielectric material and a preparation method and application thereof, and the preparation method comprises the following steps: mixing barium titanate powder, a grain growth inhibitor and a binder, and carrying out normal pressure sintering to prepare the nanocrystalline barium titanate ceramic dielectric material, the grain growth inhibitor is composed of a combination of at least two of a magnesium source, an aluminum source or a silicon source. The nanocrystalline barium titanate ceramic dielectric material is prepared by taking at least two of a magnesium source, an aluminum source or a silicon source as grain growth inhibitors through a simple solid-phase coating method, the preparation method is simple, and the prepared nanocrystalline barium titanate ceramic dielectric material can be widely applied to the field of electronic ceramics and can be widely applied to the field of electronic ceramics. The method can be particularly used for multilayer ceramic capacitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nanocrystalline material preparation, and in particular to a nanocrystalline barium titanate ceramic dielectric material and a preparation method and application thereof. Background Art

[0002] Multilayer ceramic capacitors (MLCCs), surface-mount electronic components, are widely used in various electronic products due to their small size, high specific capacitance, low dielectric loss, and high reliability. Barium titanate is the preferred material for manufacturing multilayer ceramic capacitors due to its excellent dielectric, ferroelectric, and lead-free properties.

[0003] With the advancement of intelligent, integrated, and miniaturized electronic products, there is a growing demand for MLCC electronic components that offer advantages such as high capacity and compact size. To achieve these advantages, small-particle barium titanate is required to reduce the thickness of the dielectric layer and increase the number of dielectric layers. Due to its high specific surface area, small-particle barium titanate powder exhibits high sintering activity, making it prone to grain growth during the sintering process and unsuitable for the development of ultra-thin MLCCs. Therefore, the preparation of nanocrystalline ceramics is an urgent challenge in the production of high-capacity, small-size multilayer ceramic capacitors.

[0004] Mixing glass powder and barium titanate powder and calcining them can effectively inhibit grain growth. However, most glass powders contain Bi elements that are easily volatile during the sintering process, which will significantly reduce the density of the ceramic and the dielectric properties of the ceramic, seriously hindering its application in industrial production. In addition, although the grain size can be controlled by coating the surface of the barium titanate powder with a layer of grain growth inhibitor through liquid phase coating, the liquid phase coating uses organic compounds, the production process is complicated, and the dopant content cannot be accurately controlled. At the same time, the organic carbon remaining in the barium titanate is not easy to remove and will also cause environmental pollution.

[0005] The existing technology has problems such as the inability to control grain size, affecting the dielectric properties of ceramics, and environmental pollution. Therefore, how to realize nanocrystalline barium titanate ceramic dielectric materials and ensure their performance has become an urgent problem to be solved. Summary of the Invention

[0006] To solve the above technical problems, the present invention provides a nanocrystalline barium titanate ceramic dielectric material and a preparation method and application thereof. The preparation method adopts a simple solid-phase coating method, selects at least two of a magnesium source, an aluminum source or a silicon source as ceramic grain growth inhibitors, and can effectively inhibit grain growth during normal pressure sintering. The prepared nanocrystalline barium titanate ceramic dielectric material has a small and uniform grain size and is suitable for multilayer ceramic capacitors. Moreover, the preparation method provided by the present invention has the advantages of simple process, easy operation, low raw material cost, harmlessness to the environment and suitability for large-scale industrialization, meeting the development needs of ultra-thin dielectric layers of MLCCs.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material, the preparation method comprising the following steps:

[0009] Mixing barium titanate powder, a grain growth inhibitor and a binder, and sintering at normal pressure to prepare the nanocrystalline barium titanate ceramic dielectric material;

[0010] The grain growth inhibitor is composed of at least two of a magnesium source, an aluminum source or a silicon source. Typical but non-limiting combinations include a combination of a magnesium source and an aluminum source, a combination of an aluminum source and a silicon source, a combination of a magnesium source and a silicon source, or a combination of a magnesium source, an aluminum source and a silicon source.

[0011] The preparation method adopts a simple solid-phase coating method, selects at least two of a magnesium source, an aluminum source, or a silicon source as ceramic grain growth inhibitors, and can effectively inhibit grain growth during the atmospheric pressure sintering process; the prepared nanocrystalline barium titanate ceramic dielectric material has a small and uniform grain size and is suitable for multilayer ceramic capacitors; moreover, the preparation method provided by the present invention has the advantages of simple process, easy operation, low raw material cost, harmlessness to the environment, and suitability for large-scale industrialization, meeting the development needs of ultra-thin dielectric layers of MLCCs.

[0012] Among them, the grain growth inhibitor selects at least two of the magnesium source, aluminum source or silicon source, which can better cover the surface of the barium titanate powder than using any one of them alone, thereby achieving the effect of inhibiting grain growth during atmospheric pressure sintering.

[0013] Preferably, taking the total molar percentage of barium titanate powder, Mg in the magnesium source, Al in the aluminum source, and Si in the silicon source as 100%, the molar percentage of Mg in the magnesium source is 0.1%-4%, the molar percentage of Al in the aluminum source is 0.2%-7.6%, the molar percentage of Si in the silicon source is 0.25%-0.65%, and the remainder is barium titanate powder.

[0014] The molar percentage of Mg in the magnesium source is 0.1%-4%, for example, 0.1%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] Preferably, the molar percentage of Al in the aluminum source is 0.2%-7.6%, for example, it can be 0.2%, 1%, 2%, 3%, 4%, 5%, 7% or 7.6%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the molar percentage of Si in the silicon source is 0.25%-6.5%, for example, it can be 0.25%, 1%, 2%, 3%, 4%, 5%, 6% or 6.5%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the magnesium source includes any one or a combination of at least two of magnesium oxide, magnesium carbonate or magnesium hydroxide. Typical but non-limiting combinations include a combination of magnesium oxide and magnesium carbonate, a combination of magnesium carbonate and magnesium hydroxide, or a combination of magnesium oxide, magnesium carbonate and magnesium hydroxide.

[0018] Preferably, the aluminum source includes any one or a combination of at least two of aluminum oxide, aluminum hydroxide or aluminum nitrate. Typical but non-limiting combinations include a combination of aluminum oxide and aluminum hydroxide, a combination of aluminum hydroxide and aluminum nitrate, or a combination of aluminum oxide, aluminum hydroxide and aluminum nitrate.

[0019] Preferably, the silicon source includes any one or a combination of at least two of silicon oxide, silicic acid or tetraethyl silicate. Typical but non-limiting combinations include a combination of silicon oxide and silicic acid, a combination of silicic acid and tetraethyl silicate, or a combination of silicon oxide, silicic acid and tetraethyl silicate.

[0020] Preferably, the grain growth inhibitor is a combination of a magnesium source, an aluminum source and a silicon source; as a further preferred technical solution, the grain growth inhibitor is a combination of MgO, Al2O3 and SiO2, or a combination of MgCO3, Al(OH)3 and H2SiO3, or a combination of Mg(OH)2, Al(NO3)3 and C8H 20 Combination of O4Si.

[0021] Preferably, the binder includes polyvinyl alcohol (PVA) solution or polyvinyl butyral (PVB) solution.

[0022] Preferably, the mass fraction of the solute in the binder is 2.5-10%, for example, it can be 0.2%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 3.8%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] In the present invention, the binder is removed during normal pressure sintering. The function of the binder is to facilitate granulation and tableting. The present invention does not impose any specific limitation on the amount of the binder, as long as granulation and tableting can be achieved.

[0024] Preferably, the mixing comprises first ball-milling the barium titanate powder and the grain growth inhibitor, drying to obtain porcelain powder, and then uniformly mixing the porcelain powder with the binder.

[0025] Preferably, the ball milling comprises wet ball milling.

[0026] Exemplarily, the wet ball milling uses water and / or ethanol as a solvent, and the mass ratio of the solvent to the desired wet ball milling material is (1.5-2.5):1, for example, it can be 1.5:1, 1.7:1, 1.9:1, 2:1, 2.3:1 or 2.5:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the ball mill has a rotational speed of 220-600 r / min, for example, 220 r / min, 250 r / min, 300 r / min, 400 r / min, 500 r / min or 600 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the ball milling time is 6-48 h, for example, 6 h, 12 h, 18 h, 24 h, 30 h, 36 h, 42 h or 48 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the drying time and temperature is 80-100°C, for example, 80°C, 85°C, 90°C, 95°C or 100°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the drying temperature is 6-24h, for example, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, after the mixing and before the pressureless sintering, granulation, tableting and debinding are also carried out in sequence.

[0032] Preferably, the tabletting pressure is 50-530 MPa, for example, 50 MPa, 100 MPa, 200 MPa, 300 MPa, 400 MPa, 500 MPa or 530 MPa, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the debinding atmosphere includes air or a mixed gas.

[0034] Preferably, the mixed gas includes hydrogen and nitrogen.

[0035] Preferably, the volume content of hydrogen in the mixed gas does not exceed 3 vol%, for example, it can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the heating rate for debinding is 0.5-5°C / min, for example, 0.5°C / min, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 4.5°C / min or 5°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the debinding temperature is 500-650°C, for example, 500°C, 520°C, 560°C, 600°C, 620°C or 650°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] Preferably, the debinding time is 30-180 min, for example, 30 min, 60 min, 90 min, 120 min, 150 min or 180 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the sintering atmosphere for the pressureless sintering includes air or a mixed gas.

[0040] Preferably, the mixed gas includes hydrogen and nitrogen.

[0041] Preferably, the volume percentage of hydrogen in the mixed gas does not exceed 3 vol%, for example, it can be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the heating rate of the pressureless sintering is 3-10°C / min, for example, it can be 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the pressureless sintering temperature is 1050-1225°C, for example, 1050°C, 1100°C, 1150°C, 1200°C, 1220°C or 1225°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] Preferably, the pressureless sintering time is 60-300 min, for example, 30 min, 60 min, 90 min, 120 min, 150 min or 180 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] In a second aspect, the present invention provides a nanocrystalline barium titanate ceramic dielectric material, which is prepared according to the preparation method described in the first aspect.

[0046] In a third aspect, the present invention provides an application of the nanocrystalline barium titanate ceramic dielectric material described in the second aspect, wherein the nanocrystalline barium titanate ceramic dielectric material is used for a multilayer ceramic capacitor.

[0047] Compared with the prior art, the present invention has at least the following beneficial effects:

[0048] The present invention uses at least two of a magnesium source, an aluminum source, or a silicon source as grain growth inhibitors and can prepare a nanocrystalline barium titanate ceramic dielectric material through a simple solid-phase coating method. The prepared nanocrystalline barium titanate ceramic dielectric material has small and uniform grain size and is suitable for multilayer ceramic capacitors. Moreover, the preparation method provided by the present invention has the advantages of simple process, easy operation, low raw material cost, harmlessness to the environment, and suitability for large-scale industrialization, thus meeting the development needs of ultra-thin dielectric layers in MLCCs. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 is an SEM image of the barium titanate powder in Example 1;

[0050] Figure 2 This is an SEM image of the nanocrystalline barium titanate ceramic dielectric material prepared in Example 1;

[0051] Figure 3 This is a statistical distribution diagram of the grain size of the nanocrystalline barium titanate ceramic dielectric material prepared in Example 1;

[0052] Figure 4 This is the XRD pattern of the nanocrystalline barium titanate ceramic dielectric material prepared in Example 1;

[0053] Figure 5 This is a diagram showing the dielectric properties of the nanocrystalline barium titanate ceramic dielectric material prepared in Example 1;

[0054] Figure 6 This is an SEM image of the nanocrystalline barium titanate ceramic dielectric material prepared in Example 4;

[0055] Figure 7 This is an SEM image of the nanocrystalline barium titanate ceramic dielectric material prepared in Example 5;

[0056] Figure 8 This is an SEM image of the barium titanate ceramic dielectric material prepared in Comparative Example 1;

[0057] Figure 9 This is the SEM image of the barium titanate ceramic dielectric material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0058] For the convenience of understanding the present invention, the present invention is given below with examples. It should be understood by those skilled in the art that the examples are only for the purpose of helping to understand the present invention and should not be regarded as specific limitations of the present invention.

[0059] Example 1

[0060] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material, the preparation method comprising the following steps:

[0061] (1) barium titanate powder and a grain growth inhibitor were wet ball milled at 400 r / min and then dried at 80°C for 12 h to obtain porcelain powder;

[0062] The grain growth inhibitor is a combination of MgO, Al2O3 and SiO2;

[0063] Based on the total molar percentage of barium titanate powder, MgO, Al2O3 and SiO2 being 100%, the molar percentage of MgO is 0.3%, the molar percentage of Al2O3 is 0.2%, the molar percentage of SiO2 is 0.4%, and the remainder is barium titanate powder;

[0064] The average particle size of the barium titanate powder is 100 nm, the average particle size of MgO is 40 nm, the average particle size of Al2O3 is 50 nm, and the average particle size of SiO2 is 20 nm;

[0065] The wet ball milling process uses ethanol as a solvent, and the mass ratio of the solvent to the desired wet ball milling material is 2:1;

[0066] (2) The ceramic powder obtained in step (1) was uniformly mixed with an 8 wt% PVA solution, and granulated and tableted in sequence; then, the mixture was heated to 600°C in an air atmosphere at a heating rate of 2°C / min and kept at that temperature for 150 minutes to perform binder removal; then, the mixture was heated to 1150°C at a heating rate of 5°C / min and kept at that temperature for 120 minutes to perform normal pressure sintering to obtain a nanocrystalline barium titanate ceramic dielectric material;

[0067] The tableting is performed under a pressure of 300 MPa to obtain a ceramic green body.

[0068] The scanning electron microscope (SEM) image of barium titanate powder in this embodiment is as follows: Figure 1As shown, the powder particle size is about 100nm; the 20000 magnification SEM image of the prepared barium titanate ceramic dielectric material is as shown Figure 2 As shown in the results, the ceramic is dense, the grain size is uniform, and there are no abnormally large grains; the grain statistical distribution diagram of the prepared barium titanate ceramic dielectric material is shown in Figure 3 As shown in Figure 2, the grain size range is 93-218nm, and the average grain size is 130nm. The XRD pattern of the prepared barium titanate ceramic dielectric material is shown in Figure 2. Figure 4 As shown in the figure, the results show that the ceramic is a single phase without any other impurities. The dielectric properties of the prepared barium titanate ceramic dielectric material are shown in the figure. Figure 5 shown.

[0069] Example 2

[0070] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material, the preparation method comprising the following steps:

[0071] (1) barium titanate powder and a grain growth inhibitor were wet ball milled at 220 r / min and then dried at 90°C for 6 h to obtain porcelain powder;

[0072] The grain growth inhibitor is a combination of MgCO3, Al(OH)3 and H2SiO3;

[0073] Based on the total molar percentage of barium titanate powder, MgCO3, Al(OH)3 and H2SiO3 being 100%, the molar percentage of MgCO3 is 0.1%, the molar percentage of Al(OH)3 is 0.2%, the molar percentage of H2SiO3 is 0.25%, and the remainder is barium titanate powder;

[0074] The average particle size of the barium titanate powder is 50 nm;

[0075] The wet ball milling process uses ethanol as a solvent, and the mass ratio of the solvent to the desired wet ball milling material is 1.5:1;

[0076] (2) The ceramic powder obtained in step (1) was uniformly mixed with a 2.5 wt% PVB solution, and granulated and tableted in sequence; then, the mixture was heated to 500°C in an air atmosphere at a heating rate of 0.5°C / min and kept at that temperature for 30 minutes to perform binder removal; then, the mixture was heated to 1050°C at a heating rate of 3°C / min and kept at that temperature for 60 minutes to perform normal pressure sintering to obtain a nanocrystalline barium titanate ceramic dielectric material;

[0077] The tableting is performed under a pressure of 300 MPa to obtain a ceramic green body.

[0078] Example 3

[0079] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material, the preparation method comprising the following steps:

[0080] (1) barium titanate powder and a grain growth inhibitor were wet ball milled at 600 r / min and then dried at 100° C. for 24 h to obtain porcelain powder;

[0081] The grain growth inhibitor is a combination of MgO, Al2O3 and SiO2;

[0082] Based on the total molar percentage of barium titanate powder, MgO, Al2O3 and SiO2 being 100%, the molar percentage of MgO is 4%, the molar percentage of Al2O3 is 3.8%, the molar percentage of SiO2 is 0.65%, and the remainder is barium titanate powder;

[0083] The average particle size of the barium titanate powder is 400 nm, the average particle size of MgO is 40 nm, the average particle size of Al2O3 is 50 nm, and the average particle size of SiO2 is 20 nm;

[0084] The wet ball milling process uses ethanol as a solvent, and the mass ratio of the solvent to the desired wet ball milling material is 2.5:1;

[0085] (2) The ceramic powder obtained in step (1) was uniformly mixed with a 10 wt% PVA solution, and granulated and tableted in sequence; then, the mixture was heated to 650°C at a heating rate of 5°C / min in a mixed gas atmosphere, and kept at that temperature for 180 minutes to perform binder removal; then, the mixture was heated to 1225°C at a heating rate of 10°C / min, and kept at that temperature for 300 minutes to perform normal pressure sintering to obtain a nanocrystalline barium titanate ceramic dielectric material;

[0086] The mixed gas used in the mixed gas atmosphere is a mixed gas of hydrogen and nitrogen, and the volume percentage of hydrogen is 2 vol%. The ceramic green body is obtained under a pressure of 350 MPa for tableting.

[0087] Example 4

[0088] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material. The only difference from Example 1 is that, except that the average particle size of the barium titanate powder in step (1) is 250 nm, the rest is the same as Example 1.

[0089] The 20,000-magnification SEM image of the nanocrystalline barium titanate ceramic dielectric material prepared in this embodiment is as follows: Figure 6 As shown, the results show that the grain size of the nanocrystalline barium titanate ceramic dielectric material is basically similar to that of the barium titanate powder, without abnormally large grains, and the average grain size is 265nm.

[0090] Example 5

[0091] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material. The only difference from Example 4 is that, except that the molar percentage of MgO in step (1) is 1%, the air atmosphere is replaced by a mixture of 98.5% N2 and 1.5% H2, and the sintering temperature is 1250°C, the rest is the same as Example 4.

[0092] The 20,000-magnification SEM image of the nanocrystalline barium titanate ceramic dielectric material prepared in this embodiment is as follows: Figure 7 As shown, the results show that the grain size of the ceramic is basically similar to that of barium titanate powder, without abnormally large grains, and the average grain size is 278nm.

[0093] Example 6

[0094] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material. The method is the same as that of Example 1 except that MgO in the grain growth inhibitor is replaced with Al2O3 and SiO2 in a molar ratio of 2:4.

[0095] Example 7

[0096] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material, which is the same as that of Example 1 except that Al2O3 in the grain growth inhibitor is replaced with MgO and SiO2 in a molar ratio of 3:4.

[0097] Example 8

[0098] This embodiment provides a method for preparing a nanocrystalline barium titanate ceramic dielectric material, which is the same as that of Example 1 except that SiO2 in the grain growth inhibitor is replaced with MgO and Al2O3 in a molar ratio of 3:2.

[0099] Comparative Example 1

[0100] This comparative example provides a method for preparing a barium titanate ceramic dielectric material, which is the same as Example 1 except that MgO, Al2O3 and SiO2 are not added in step (1).

[0101] The 20000 magnification SEM image of the barium titanate ceramic dielectric material prepared in this comparative example is as follows Figure 8 As shown, the results show that the average grain size of the ceramic is 1.32 μm.

[0102] Comparative Example 2

[0103] This comparative example provides a method for preparing a barium titanate ceramic dielectric material. The only difference from comparative example 1 is that, except that the particle size of the barium titanate powder in step (1) is changed to 250 nm and the sintering temperature in step (3) is 1250° C., the rest is the same as comparative example 1.

[0104] The 20000 magnification SEM image of the barium titanate ceramic dielectric material prepared in this comparative example is as follows Figure 9 As shown, the results show that the average grain size of the ceramic is 1.95 μm.

[0105] Comparative Example 3

[0106] This comparative example provides a method for preparing a barium titanate ceramic dielectric material, which is the same as Example 1 except that equal molar amounts of Al2O3 and SiO2 are replaced by MgO.

[0107] Comparative Example 4

[0108] This comparative example provides a method for preparing a barium titanate ceramic dielectric material, which is the same as Example 1 except that MgO and SiO2 are replaced by Al2O3 in equal molar amounts.

[0109] Comparative Example 5

[0110] This comparative example provides a method for preparing a barium titanate ceramic dielectric material, which is the same as Example 1 except that MgO and Al2O3 are replaced by SiO2 in equal molar amounts.

[0111] Test Method

[0112] The average grain size of the barium titanate ceramic dielectric materials prepared in Examples 1-8 and Comparative Examples 1-5 was measured using a scanning electron microscope (SEM) at different magnifications. The results are shown in Table 1:

[0113] Table 1

[0114]

[0115]

[0116] The test results show that:

[0117] (1) It can be seen from Examples 1-3, Examples 6-8, and Comparative Examples 1-5 that the present invention uses magnesium, aluminum, and silicon elements as grain growth inhibitors and can prepare nanocrystalline barium titanate ceramic dielectric materials with small and uniform grain sizes through a simple solid-phase coating method;

[0118] (2) It can be seen from Examples 1 and 4 that the present invention can further optimize the grain size of the nanocrystalline barium titanate ceramic dielectric material by further controlling the particle size of the barium titanate powder.

[0119] (3) It can be seen from Examples 1 and 6-8 that the present invention can further optimize the particle size of the nanocrystalline barium titanate ceramic dielectric material by controlling the amount and type of the grain growth inhibitor.

[0120] In summary, the present invention uses at least two of a magnesium source, an aluminum source, or a silicon source as grain growth inhibitors, and can prepare a nanocrystalline barium titanate ceramic dielectric material through a simple solid-phase coating method. The prepared nanocrystalline barium titanate ceramic dielectric material has a small and uniform grain size and is suitable for multilayer ceramic capacitors. Moreover, the preparation method provided by the present invention has the advantages of simple process, easy operation, low raw material cost, harmlessness to the environment, and suitability for large-scale industrialization, thereby meeting the development needs of ultra-thin dielectric layers of MLCCs.

[0121] The applicant declares that the above is only a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention fall within the scope of protection and disclosure of the present invention.

Claims

1. A method for preparing a nanocrystalline barium titanate ceramic dielectric material, characterized in that: The preparation method comprises the following steps: Mixing barium titanate powder, a grain growth inhibitor and a binder, and sintering at normal pressure to obtain the nanocrystalline barium titanate ceramic dielectric material; The grain growth inhibitor includes at least two of a magnesium source, an aluminum source, or a silicon source.

2. The preparation method according to claim 1, characterized in that Taking the total molar percentage of barium titanate powder, Mg in the magnesium source, Al in the aluminum source, and Si in the silicon source as 100%, the molar percentage of Mg in the magnesium source is 0.1%-4%, the molar percentage of Al in the aluminum source is 0.2%-7.6%, the molar percentage of Si in the silicon source is 0.25%-0.65%, and the remainder is barium titanate powder.

3. The preparation method according to claim 1, characterized in that The magnesium source includes any one of magnesium oxide, magnesium carbonate or magnesium hydroxide, or a combination of at least two thereof; Preferably, the aluminum source comprises any one of aluminum oxide, aluminum hydroxide or aluminum nitrate, or a combination of at least two thereof; Preferably, the silicon source includes any one of silicon oxide, silicic acid or tetraethyl silicate, or a combination of at least two thereof.

4. The preparation method according to any one of claims 1 to 3, characterized in that The binder includes a polyvinyl alcohol solution or a polyvinyl butyral solution; Preferably, the mass fraction of the solute in the binder is 2.5-10%.

5. The preparation method according to any one of claims 1 to 4, characterized in that The mixing comprises first ball-milling barium titanate powder and a grain growth inhibitor, drying to obtain porcelain powder, and then uniformly mixing the porcelain powder with a binder; Preferably, the ball milling comprises wet ball milling; Preferably, the ball milling speed is 220-600 r / min and the time is 6-48 h; Preferably, the drying temperature is 80-100° C. and the drying time is 6-24 hours.

6. The preparation method according to any one of claims 1 to 5, characterized in that After the mixing and before the pressureless sintering, granulation, tableting and debinding are carried out in sequence; Preferably, the tabletting pressure is 50-530 MPa.

7. The preparation method according to claim 6, characterized in that The heating rate of the debinding process is 0.5-5°C / min; Preferably, the debinding temperature is 500-650°C; Preferably, the debinding time is 30-180 minutes.

8. The preparation method according to any one of claims 1 to 7, characterized in that The sintering atmosphere of the pressureless sintering includes air or a mixed gas; Preferably, the mixed gas comprises hydrogen and nitrogen; Preferably, the volume percentage of hydrogen in the mixed gas does not exceed 3 vol%; Preferably, the heating rate of the pressureless sintering is 3-10°C / min; Preferably, the pressureless sintering temperature is 1050-1225°C; Preferably, the pressureless sintering time is 60-300 min.

9. A nanocrystalline barium titanate ceramic dielectric material, characterized in that: The nanocrystalline barium titanate ceramic dielectric material is prepared by the preparation method according to any one of claims 1-8.

10. An application of the nanocrystalline barium titanate ceramic dielectric material according to claim 9, characterized in that: The nanocrystalline barium titanate ceramic dielectric material is used for multilayer ceramic capacitors.